Started by Trudi, October 06, 2010, 01:23:58 PM

Previous topic - Next topic

0 Members and 2 Guests are viewing this topic.

Trudi

Hi

I do some fusing but not much - and I don't have a problem normally when cutting - but I'm usually cutting from smaller bits of glass.

Recenltly I bought some sheet glass 3mm 25x25cm - some cut ok (not brilliant) and some did not break along the line. I checked my cutter on a smaller piece of glass and it's fine.

Is it more tricky because it's a bigger piece of glass?

I'm using  plastic running pliers - http://www.warm-glass.co.uk/Shop/ProductDetails.aspx?ProductId=284 and a toyo cutter http://www.warm-glass.co.uk/Shop/ProductDetails.aspx?ProductId=275

any tips appreciated!

Trudi x

hollergrafik

Trudi, are you standing up when you cut it?


Margram

And are you cutting from the middle of the sheet i.e. the first cut down the centre of the sheet, the next down the centre of one of the ensuing pieces etc? Link here - see point 3: http://www.warm-glass.co.uk/Information/Studio.aspx :)
Marg x  Etsy Flickr My blog

LittleHen

Are you cutting long runs of thin strips?  If so them maybe a small fault/air bubble/inperfection will make the cut run to the nearest edge.  Could you cut the big bits into smaller bits before cutting strips off?
It's harder to cut a long inch strip off a big bit than it is to cut the big bit in half.  It's like electricity and water, the cut always takes the shortest route!
I used to do stained glass and cutting big bits is easy but smaller bits I hated!  
Hope that helps
Jessie

Krysia@No98


I have a similar problem cutting glass.  I check

1. standing up and bearing down with all my weight.  Trying to make sure I apply continuous pressure
2. enough oil on/in the cutting blade
3. I am using a cutting mat
4. it's making the right kind of noise when I am moving the blade
(5. no ones looking when I do it  ;))

HTH
-* -  Courage is going from failure to failure with out loosing enthusiasm -*-

Trudi

Hi

I'd bought a sheet of effetre glass 25x25cm - and I was wanting to make my own streamers and fractures (instead of buying the pre-made BE ones). I thought the 104 would be good as I have loads of murrini and shards and can pull stringers .

I was trying to cut the glass into 4 10x10cm bits with a small off cut (Ideal for pendants). I just wasn't getting clean cuts like I do with smaller pieces. I thought perhaps the glass was thicker - it's 3mm so I tried cutting a smaller piece of 3mm BE - worked fine. So then I wondered if I need better running pliers??

I'm glad it was only plain glass and not expensive (I'm still managing to use it for the dicro tabs I'm making for stringers - so no loss) but I'm glad I didn't order a big sheet of patterned glass and ruin it.

I just want to understand what I'm doing wrong ......... Dawn I'm going to have to write myself a wish list for one of your classes. I'd really like to start understanding it all a bit more!

PS - I have just topped up the oil, and have a cutting mat (couldn't cut without it).

I haven't done much cutting or fusing to be honest. Just over a year ago I went on a basic fusing course which covered the basics as I have an SC2 kiln. So it's not big time fusing I'm after, but might as well make the most of the kiln and I've enjoyed the bits I've done so far and love the coasters/candle mats.

Zeldazog

All good tips here, and honestly not sure what the answer is.  I haven't used Effetre sheet glass, so I don't know what it's like in terms of texture - the more textured it is, the harder it is to cut - but Bullseye colours are hand-rolled too, so that's not necessarily the problem.

When you say you're not getting clean cuts, do you mean it's going off line, or its just got a nastier edge?

To be honest, I don't use cut runners on large pieces, unless it's a strip off the edge.  I find the following two ways more effective:

1) Take score line to the edge of your cutting mat/carpet edge so that one half is hanging over the edge - so there's a height difference.  Press firmly with the flat of your hand on the bit that has a bit space behind it (on the lower side).  This only works if your score line is really good and clean.

2) (and my preference) Flip the glass over.  Place your thumbs ON the score line, one in front of the other, normally about an inch apart.
  On a surface with give, press down.  Honestly you won't cut yourself, if both your thumbs are ON the line.  If it's a really long cut, you can do this along the line in several places, working from one end to the other.

Effective cutting is something that takes time, and some colours are easier to do than others - I dislike cutting Bullseye white for example, it never plays nicely for me.

One question, Trudi - are you trying to break the glass AS SOON as you've done each score line? 

Trudi

Hi thanks for the replies

Dawn - the break starts off ok then at one end I get rough edges.

And yes I do break as soon as I've scored!

Zeldazog

In that case, I'd suggest you try one of the other breaking methods - cut runners are only applying pressure at one end, which where I presume it's okay - by the time you get to the far side of the glass, they aren't really applying the same pressure anymore - at least, that's what I would guess.

♥♥Tan♥♥

What about the good old HIIIIIYAAAAA karate chop method? Shatters it to a squillion pieces but its sooo satisfying to make that noise

Krysia@No98

if you could record a little clip and post it on youtube Tan, that would be great, you know so we can see how it's done  ;D
-* -  Courage is going from failure to failure with out loosing enthusiasm -*-

dinah46

I use the morton safety break and can really recommend it, http://www.tempsfordstainedglass.co.uk/acatalog/Accessories.html, it's good for strips and curves and makes a really clean cut.

However, I have a sheet of bullseye black that defies all attempts to cut clean strips so sometimes you can definitely blame the glass :)

Trudi

Quote from: Tan on October 06, 2010, 06:17:18 PM
What about the good old HIIIIIYAAAAA karate chop method? Shatters it to a squillion pieces but its sooo satisfying to make that noise

Tan did you go to the Hong Kong Fooey School of glass cutting - I like your style crazy woman!!

And thanks for the info Diane - I shall investigate later when I'm fully awake! It could be partly the glass but I do wonder if it's also because it's a bigger area and my pliers are only basic ones - which have served me well thus far!

Thanks guys for all the tips - you're all great!

dinah46

Are you going to Di's open day tomorrow Trudi, if you are I could bring the morton thingy with me for you to see how it works.  I also have a different style of running plier that works well.