GlassOwl

Hi folks

I have been asked by a friend of mine if I could make her daughter a "girly pink" pendant and bracelet for Christmas.

Not had a lot of experience with pinks and not sure what would be the ebst colours to go for.

Any advice would be gratefully received

Thanks

Sandra

Helen G

Hi Sandra

I like effetre 256 and 260 with touches of Rubino. I find the opaque pinks like to be worked quite cool and struck to get the best out of them as does Rubino of course   ;)

This is 256 I think?! with tiny Rubino dots on the flowers.


♥♥Tan♥♥

Wot she said.........and very beautiful beads by the way ;) :D

Trudi

There is a themed S&T for pinks see here http://www.frit-happens.co.uk/forum/index.php?topic=7720.0

This may help - if you find a shade you like you can always ask what colour it is.

My neice is pink daft, but she really likes deeper pinks like Rubino or pink lady.

Trudi

Another thought  - if you go into the Frit Happens Group on Flicker and search for pink http://www.flickr.com/search/groups/?q=pink&w=744927%40N24&m=pool

you get some nice beads - and I'm sure if you found some beads you liked, people here would be able to suggest what colours were used.

MadelineBunyan

cim gellys sty is a girly pink.

effetre baby pink is nice, but I tend to just use their light pink cause its not much lighter, but alot cheaper!

for a transparent I like cim blush, good over white sparkle pixie dust & czs.

Lilley

I was making pink beads recently - and struggling!  I now know that rubino reacts with some other colours and goes black and horrid - I think it was purple and ivory that caused most problem (bit of a shame as the person wanted a pink and purple bead).  Also I found that Reichenbach opal raspberry didn't play nicely for me (but I am relatively new to this game).  I did eventually make a suitable bead, but stupidly didn't note the name so that's not much help - it was an effetre pink though and not cheap!!  Personally, I've gone off pink!
Glass - lampworked, blown, kilncast or fused and slumped, it's all good!
website: http://lilleyglassdesigns.co.uk/

GlassOwl

Thank you folks

I am ordering new pinks to make these beads

Many thanks

Sandra

helenfc

i am so not a pink person, but those are gorgeous helen :) what pinks did you go for sandra?

GlassOwl

HI

Great information everyone and thanks

I bought 256 and 260 and restocked my rubino oro

Hopefully I can play this weekend or next

Thanks for your help

Sandra

Trudi

Hi with rubino - it's best to work in a neutral flame - if you're on a hot head just work a little further out!