Main Menu

'Silver Brown' conundrum

Started by Clair, March 20, 2010, 08:40:03 PM

Previous topic - Next topic

0 Members and 1 Guest are viewing this topic.

Clair

I found some rods of a glass which has the label 'silver brown' on it. I bought it so long ago, I can't even remember which make of glass it is. The problem is, that no matter what I do with this glass, it melts into clear - no colour, no irridescence, nothing!
I've tried reducing it; oxidising it; cooling it to within an inch of its life and quickly reheating it; using it with frit and silver - it stubbornly refuses to react or reduce and just bleaches to a clear glass.
The rod is a transluscent brown with stratas of dark and pale brown in.
Does anyone have any idea what this glass is and what I should do to tease it into life?

Veebee

Souds about right. It's Reichenbach and it's tricky! Get the shape, cool, reduce, then encase REALLY slowly. The silver will disappear if it is over heated on encasement.
HTH!
Web: http://www.veebeads.net
The UK home of Val Cox frit!!
Fritt Flickr group: http://www.flickr.com/groups/1647822@N25/

Clair


Veebee

Web: http://www.veebeads.net
The UK home of Val Cox frit!!
Fritt Flickr group: http://www.flickr.com/groups/1647822@N25/

Trudi

If you do a search, probablyin s&t, you'll find a thread about it!

silverlemon

Hi Clair, this glass strikes and reduces.

I tend to pull stringers from it, it goes clear when I get it hot enough to pull a stringer.

Try it over red, cobalt  or ink. You need to reduce heavily, then encase. While you melt your encasing in it will naturally strike.


I've also seen it used on ivory and reduced, looked yummy.

HTH  :)

Bionic Sarah xxx    Sarah Downton On Facebook  My Etsy Shop

Clair

Thanks Sarah and Trudi for pointing me in the direction of S&T (sounds like a dubious yet pleasurable practice!) I'll give it a go again as I obviously haven't reduced it enough. Must admit, I never thought to encase it either!  :P

♥♥Tan♥♥

Fab tips Sarah, I'm about to have a play for the first time and your bit about the stringer going clear has set me on the right track

Trudi

Quote from: Clair on March 22, 2010, 08:26:08 PM
Thanks Sarah and Trudi for pointing me in the direction of S&T (sounds like a dubious yet pleasurable practice!) I'll give it a go again as I obviously haven't reduced it enough. Must admit, I never thought to encase it either!  :P


ahhhhhhhh it's all in the encasing!

helenfc

aaah this is handy, i found dark silver brown quite easy, then ordered silver brown instead (whoops) and found it really hard to work with! thanks! :)

Krysia@No98



I've made some discs with it.  Personally I quite like it as it is, but then I'm funny like that  ::)
-* -  Courage is going from failure to failure with out loosing enthusiasm -*-

Clair

Quote from: Krysia on March 24, 2010, 03:24:51 PM


I've made some discs with it.  Personally I quite like it as it is, but then I'm funny like that  ::)

Have you got any piccies?

Krysia@No98

#12
I do, but it's made up into a necklace so it's kind difficult to make out....  Let me fiddle and see what I can do...



It's not great I'm afraid.  I would take another picture but it was a christmas pressie  :-\
-* -  Courage is going from failure to failure with out loosing enthusiasm -*-

fionaess

This is silver brown, reduced and then encased...





If it's got a hole, it's a bead !

julieHB

Julie xx

                           My Webbie - My Flickr