Hi, I bought a rod of Multicolour glass to try out this week.
Made quite a nice bead from cobalt blue with some multicolour trailed around it - but the multicolour just looks a dull pale green now that it has cooled (not annealled yet , Beadcube only arrived today and I haven't worked out how to use it yet!  :D).

I was hoping for...well, colours - I am on a Hothead, can anyone tell me how to get better results?
Thanks!

helbels

You need to strike it.

You CAN definitely do it on a Hothead (I've done it).

Heat it up until very hot (as hot as you can go), then take it out of the flame and cool it until the glow is gone (check it under your bench as its darker there).  Gradually reintroduce it to the very tip of the flame, and you will see the colours start to appear!

Good luck....

Helen G

I find it likes lot of marvering especially with brass then heating again and mavering etc etc

Kaz

And you's be so much better off with multicolour dark as it is much easier to get reactions out of.
Kazx
She's made of real glass. She got real real emotion. But my heart laughs I have that same sweet devotion!

Helen G

Quote from: Kaz on August 13, 2010, 10:42:33 PM
And you's be so much better off with multicolour dark as it is much easier to get reactions out of.
Kazx

Ah! I thought that's what we were talking about, not used regular multicolour  :-[

Trudi

I found that the more you use the better - I made some 16mm rounds - and as you naturally have to heat and cool as you add more glass it strikes as you make the bead  - I think the same would be true when Sabine made roses out of it!

And it looks fabaroony etched!

cbeadies

Thanks everyone!
I'll try again tomorrow and follow the advice given. I'm determined to get some colours out of it now!

Shirley

I find you have to be patient with it. When I reintroduce it to the flame I only let it get to a dull orange glow, then bring it out again. Sometimes you can see a 'bloom' moving round the bead when it's in the flame and this seems to be when the colours develop. I love it.
Val Cox Frit - Thai and Bali Silver 

metaltedgrrl

I also find it changes again slightly in the kiln...good luck!
Trying harder every day!

stuwaudby

I usually have trouble getting a good strike in the flame. It tends to strike at a very low temperature, if you get any glow on the bead you may loose the strike.

I get by far the best colours when they kiln strike during batch annealing. If not then try lifting the anneal temperature 25 degrees to help it.

You can get a great effect with multicolour by mixing it with clear, about 4 to 1 and making clear beads. When they are flamed they look like yellow tinged clear. After annealing they are amazing. The following was annealed for 1 hour @ 512 DEgC, sorry about the photo quality:



Stu

Trudi

you'ver really got some nice effects going on there!

Maria Louisa

Thank you for that tip Stu, I'm certainly gone try that one out. That beads is beautiful.
www.glassbeadsculptress.com
www.glassbeadsculptress.etsy.com
www.beadpress.nl
www.flickr.com/beadpress

kathsd

nice colours in that bead Stu,
I will have to try again, yesterday I made some clear lentils encased with multi, but could only get greens and blues, I can't have been striking it enough, or possibly too much? but then again when I tell you that I couldn't work out where the colour had gone from my CIM pheonix beads (until I found some older posts   ::))as they were turing out colourless!! , so my next session will be trying out some more striking, and I've just watched Laura Sparling's tutorial on youtube, so I should be sucessful (fingers crossed!!)  :)
kath

loribeads

Beautiful bead, Stu!  I have had pretty good luck using Multicolor or Dark Multicolor in twisties (usually with just black or clear).  I think it's because I am getting the Multi hot during the twisty making process and then again when adding to the bead, thus striking the color fairly well. 
Murrini:  www.loriandkim.com 

Beads:  www.loribeads.etsy.com

Redhotsal

I got absolutely ZILCH out of the Multicolour batch that I bought a few months ago. It wasn't the dark one but I do remember reading on here that some people had some multicolour that did very little. So, if you've tried and tried and got nothing it MAY be the batch you have.