Firepolish schedule for Dichroic glass

Started by spexy, December 17, 2014, 08:14:51 AM

Previous topic - Next topic

0 Members and 1 Guest are viewing this topic.

spexy

I've been searching for a firepolish schedule for 104 dichroic glass. I have a couple of strips that need doing and I can't find one. I'd also like to try fire polishing some of my Bullseye dicrho into strips so I need a schedule for that.

Can anyone point me in the right direction please?

Trudi

Hi

This is what I use (SC2 kiln)

Fire Polish
Ramp-temp-hold
300   600   0
500   735* 10
900   516   15
80     371   10
0


hope that helps


spexy

Thanks Trudy, is that the same for both COE's

Trudi

I've used it on both ... You may need to tweek if your kiln runs differently from mine, so it may be best to test a small bit first!