Grey streaks on light turquoise beads

Started by Donna@Rockin' Beads, December 31, 2010, 09:29:58 AM

Previous topic - Next topic

0 Members and 1 Guest are viewing this topic.

Donna@Rockin' Beads

I made a whole load of turquoise beads and they practically all have silvery grey streaks on them. I am on mains gas and am assuming that I reduced the glass but I am certain my flame was ok.

Any thoughts?

Thanks

Les

It does sound like a bit of reduction Donna ... I get it too sometimes, even with a neutral flame

Pat from Canvey

Try etching one bead and see if you like the result. If you do, go for it.

Lotti

I had a problem with dark turquoise and etched them and the streaks just disappeared like magic! :)

Donna@Rockin' Beads

The mains gas flame is not quite so obvious but I'll give myself some really pointy candles and try again!!!
I did try dipping in silver cleaning fluid but that didn't get rid of it.
I might try etching, thanks for the suggestion Pat, and Lotti  :)

Redhotsal

If you just etch for about a minute that should get rid of the grey but still leave the beads shiny. You may have to experiment with the time a little.

Lotti

Interesting Sal.  I didn't think it was working to start with so left them in for some time, they are very nice, but of course with the etch look, would have been nice to have kept them shiny, I guess after a minute when you wash them the streaks come off? :)

Les

I have heard that soaking overnight in full fat coca cola can also help to get rid of the nasty grey. Never tried it myself though

Lush!

If I want to brighten up turquoise but keep it shiny I literally dip it in the etching fluid, really quick, in and out - then neutralise with bicarb and rub it under the tap, the streaks should rub off, if not, dip again.


www.lushlampwork.etsy.com

Lilley

coca cola works well - I use the cheapest available and leave them in until all grey has gone, it can take a while (in the case of copper green gone grey = days) but the grey sludge does go eventually.  I do change the cola from time to time - I think it is the acid in it that does it and I gather some tiolet cleaners will do the same but I've not tried that.
Glass - lampworked, blown, kilncast or fused and slumped, it's all good!
website: http://lilleyglassdesigns.co.uk/

Calico Cat

I've found that Cillit Bang - Grime & Lime variety - works well but, as with the Cola, you may have to leave the beads in for a while.


Watch this space for new Etsy shop . . .

Lotti

I tried cilit bang and it didn't work, but maybe I should have left them in longer.  :)

Kaz

Cilit Bang Lime and Grime and leave in for quite a while - completely cured a set of turquoise bullseye beads for me without taking away the shine.
Kazx
She's made of real glass. She got real real emotion. But my heart laughs I have that same sweet devotion!

Helen G

Silver dip if you happen to have some does a good job too in just a minute or so  ;D

Dragonfire Glass

Cilit Lime & Grime does the trick & keeps the shine  :)