I have been starting to lampwork and I have been getting brown stains in my beads. In fact white just goes black. I have an oxycon that was sent back and re-serviced. they said it works perfectly now. I met a lampwork tutor who showed me how to set up and made a basic encased bead. I did everything she taught me at home, stil I have brown stained beads. I have fiddled with the pressures of the oxygen and propane. I have tried leaving the oxycon running with the torch open for 10 mins before lighting. I have cleaned the rods with acetone, I have tried working in every part of the flame and in every degree of flame from reducing to soft. I am at a loss for what else to try. Could it be the torch is no good? could there be something wrong with the propane? Any body have any advise or ideas? please

Redhotsal

It sounds like reduction or even burning - but a piccy of your affected beads would be helpful....

stuwaudby

Is the problem in clear glass?

Clear 104 glass can absorb carbon from a reducing flame and leave black/brown streaks.

The bottom of a gas bottle contains a higher proportion of mercaptan sulphurs which might cause discolouration.

Dirt on the glass can leave diposits behind.

Some glass just seems prone to it I am afraid. I have received glass before which contained a brown streak through the centre of the rod, highly annoying.

Sounds like you have tried everything with oxygen/gas mixture, try some different glass.

Stu