Passionatelamper

Could someone pullease......give me the program to fuse glass in the Bead cube... I put a load in yesterday... dived to the kiln this morning. All still the same as when it went in...Bah!!!! Please .......need the exact program for the bead cube....I am desperate.... ::) ;D ;)

etsy-header-dec12 by vonnie.t, on Flickr

cbeadies

 :) Sorry I don't know about fusing schedules, although I would quite like to know too as I also have a beadcube... just wondering whether Lee at Kilncare could help, they are usually very helpful there.

aercraft

I've just been doing exactly this - will dig out the programme.  Are you using bullseye?
Anne

Passionatelamper

#3
I am using Dichroic Glass to make cabs thank you  ;D I have sent an email to Brian at Kilncare but no reply yet :-}

etsy-header-dec12 by vonnie.t, on Flickr

aercraft

This is the programme I used last for Bullseye:

  1. ↑ 222 to 670, hold 20min
  2. FULL to 804, hold 10min
  3. FULL to 482, hold 30min
  4. ↓ 80 to 371, no hold
  5. FULL to 93, no hold
  6. End

Step 1 is a bubble squeeze and only short as I was doing small pieces.  The temps and times are based on the info on the Bullseye site and I got some good results with this programme.  Takes 9 hours.
Anne

Passionatelamper

Thank you soooo so much I will do that many many thanks... ;D :-*