Shirl

I used CIM blackcurrant base, wrapped in silver leaf, swiped with Triton and encased in Eff 006 clear. Then squished with my mashers as I dont have a press. (yet)

My schedule in my Paragon SC3 with bead door was



Segment 1: Ramp1 990 deg C Temp1 510 deg C Hold1 12 HRS

Segment 2: Ramp2 FULL Temp2 520 deg C ** Hold2 1 HR

Segment 3: Ramp3 50 deg C Temp3 370 deg C Hold3 0000mins

Segment 4: Ramp4 0000


turnedlight

 I dunno.. maybe it could be too much silver in your beads, in the reduction of the Triton, added to the silver foil? In the past I've had the occasional cracks with a really metallic shiny encased Triton bead, (I encase in 006 like you) and wondered if there's such a thing as too much silver!
I garage my beads, I go straight to 520, hold it there whilst adding beads in, then at the end I leave it for 30 mins to an hour depending on the beads and ramp down. I've not tried garaging at 510, it doesn't sound too low but maybe you could try going straight to 520.
kathryn

Veebee

I hold for a while after bringing down through the stress ranges, I would suggest your hold 3 should be for maybe 20 mins just to let them settle. Also, were they cool when you got them out of the kiln? (sorry if that seems to be a condescending question, it's not meant to be!) The centre of the bead holds the heat, if the bead was still warm on the outside when it went into the water then it will probably still have been warmer than you think on the inside... just another thought.
Web: http://www.veebeads.net
The UK home of Val Cox frit!!
Fritt Flickr group: http://www.flickr.com/groups/1647822@N25/

turnedlight

Ooh yes, I missed that, it's not stopping at 370 and letting the stresses even out.
kathryn

Shirl

This was the schedule for the first batch from fritpedia

Good for COE 90 and 104 glass

Segment 1: Ramp1 900 deg C Temp1 500 deg C Hold1 12 HRS

Segment 2: Ramp2 FULL Temp2 520 deg C ** Hold2 1 HR

Segment 3: Ramp3 78 deg C Temp3 370 deg C Hold3 0000mins

Segment 4: Ramp4 0000


For the second batch I changed ramp 3 to 50 deg  instead of 78 as I thought the slower cooling might be better.

I did not know you had to hold  at 370 deg. I thought it just cooled down naturally from there. The beads were left overnight so should have been well cooled

Veebee

I would definitely hold for a short while at 3, then you can just let the natural cooling happen.
Web: http://www.veebeads.net
The UK home of Val Cox frit!!
Fritt Flickr group: http://www.flickr.com/groups/1647822@N25/

Shirl

Quote from: Veebee on March 11, 2011, 05:58:52 PM
I would definitely hold for a short while at 3, then you can just let the natural cooling happen.

Thanks Veebee, it wont hurt to try that, and fingers crossed it might work :)

sarah t

we will get you there in the end  ;)

Shirl

Oh I hope so  ;D

I think I might try doing some simple test beads in different colours to see how they work out

Veebee

Lentils, of course..........
;D
Web: http://www.veebeads.net
The UK home of Val Cox frit!!
Fritt Flickr group: http://www.flickr.com/groups/1647822@N25/

Pat from Canvey

I'm not sure why you have the Segment 1 at all. I go straight to 520C ramping at FULL. After the last bead goes in, I hold for an hour, skip the program and then ramp down. Down takes 3 hours or so after the skip. No problems with any sort of bead including very large ones. I programmed mine from the manual that came with the SC2 kiln. Take beads out at about 65C hold for a few minutes to admire and then dunk in water.

Shirl

Quote from: Pat from Canvey on March 15, 2011, 11:52:30 AM
I'm not sure why you have the Segment 1 at all. I go straight to 520C ramping at FULL. After the last bead goes in, I hold for an hour, skip the program and then ramp down. Down takes 3 hours or so after the skip. No problems with any sort of bead including very large ones. I programmed mine from the manual that came with the SC2 kiln. Take beads out at about 65C hold for a few minutes to admire and then dunk in water.

Thanks Pat. :)
If I ramp at full my kiln overshoots and ends up at about 550, so I just heat up a bit slower.

I expect there are lots of ways to do it, all being a different variation.