Cracked beads

Started by Shirl, March 09, 2011, 11:47:54 PM

Previous topic - Next topic

0 Members and 2 Guests are viewing this topic.

Shirl

I usually batch anneal, but for the first time this morning I put my kiln on and garaged and then annealed as I wanted to make some hand shaped lentils and they cracked if cooled in the vermiculite when I have made them on previous sessions.

NOT a good result today, just got them from the kiln and found most of the lentil shapes cracked :'( :'(   The round beads I made at the same time were all fine.

I am not sure why this happenned. Did I get them too cool while shaping?




Veebee

Aw, gutting. Yup, that's a thermal crack, and it means you let them cool too much when shaping. After pressing/shaping etc, give the bead a good heat bath to a dull glow to help avoid this, but not so hot that the glass goes gloopy and loses shape. Have another go, they're looking good!
Web: http://www.veebeads.net
The UK home of Val Cox frit!!
Fritt Flickr group: http://www.flickr.com/groups/1647822@N25/

sarah t

cracks like that are usually thermal so ''got to cool when shapping''  or adding layers a good shout i reckon ....

the remedy is a bit tricker as i am not sure when its cooling to much ......

dont press/squish for too long ...i use the press bottom to shape and only do a final press using the top (if it has one) once if possible !...re heat in between each shapping or adding more glass but not to much or you lose the shape ...after the final press and its ready for the kiln i heat it up again in the top of the flame and give it a final bit of heat ......make sure you remember the top and bottom of the bead as well as the back and front ...i kind of rock the bead to and fro but that could just be me !

the other reason is could be they are too thin...a little less squishing could help

its also sometimes tricky to get the core back to a compatable heat when encasing ...so maybe try doing the shaping without encasing till you have had a bit more success ...

i am afraid its practise practise practise ........ but it will suddenly click ...and garaging is usually a bit more forgiving than other forms of cooling with bigger beads...shame they were looking good

good luck  


Shirl

Thanks so much for the advice :) :)

I have had another go today, but was a bit paranoid about letting them get too cool, so much so that one of my beads must have been a bit too hot and it stuck to another one as I put it in the kiln :o

Another lesson learnt

turnedlight

You don't have to wait for the glow to go completely before putting them in the kiln - just hold it so it is off the floor for a few moments til the glow goes and then you can put it down. I do this especially with the bigger beads.
kathryn

Shirl

Quote from: turnedlight on March 10, 2011, 04:51:35 PM
You don't have to wait for the glow to go completely before putting them in the kiln - just hold it so it is off the floor for a few moments til the glow goes and then you can put it down. I do this especially with the bigger beads.

I never thought of this...thanks :)

♥♥Tan♥♥

what a shame, there are some lovely beads there :'(

Margram

If you clean them really well you can slump them into lovely cabs...
Marg x  Etsy Flickr My blog

TheJanie

Quote from: Margram on March 10, 2011, 10:20:33 PM
If you clean them really well you can slump them into lovely cabs...

That's what I've been mostly doing this week :)

Lush!

Oh what a shame  :(

What size are your mandrels? They look quite thick, which would mean that the glass either side is thinner. It may help to use a finer mandrel - I use 1.6mm with my lentil press.


www.lushlampwork.etsy.com

Shirl

Quote from: Lush! on March 10, 2011, 11:03:52 PM
Oh what a shame  :(

What size are your mandrels? They look quite thick, which would mean that the glass either side is thinner. It may help to use a finer mandrel - I use 1.6mm with my lentil press.

These were made on my new 1.6 mandrels :o

Shirl

Well ......I just got my beads from the kiln this morning and I only tried one lentil ( the same glass and style as the last cracked ones for comparison) and some other round beads.......YEY no cracks, so I spent a bit of time looking at my creations and then them put them into water to remove the mandrels...... I let them soak a few mins and when looking at my lentil .....OH NO.. it is Cracked :'(  in exaxctly the same way as the last ones!

I put it in the kiln while it was quite hot, and took great care to make sure it was heated through before putting it in.

I thought I had done everything right this time....but no joy.

At least I only got one cracked! (but I only made one lentil)

If I carry on like this I will have so many half beads i will have to make them into cabs (scary) or stick them round a picture frame!

TheJanie

Quote from: Shirl on March 11, 2011, 10:38:32 AM
If I carry on like this I will have so many half beads i will have to make them into cabs (scary) or stick them round a picture frame!

I thought slumping them into cabs was scary - then finally got the courage to start experimenting this week.  I'm still trying to get the program right, but I'm getting there!

Before that, I stuck magnets on the back of half-beads and decorated my fridge with them :)

sarah t

bugger  >:(
dont know what to suggest now ....maybe different glass ??..could be a compatabilty /heat issue  ?...you could try making a few in just one type of glass

or maybe kiln ???...what temperature /schedule are you using ?


turnedlight

What glass are you using?
kathryn