Silver Leaf/Foil and subsequent fuming

Started by AnnaSpanna, November 12, 2010, 02:30:42 PM

Previous topic - Next topic

0 Members and 1 Guest are viewing this topic.

AnnaSpanna

I have a commission to do which requires me to make 5 teeny weeny round beads as part of it. They need to have a silver foil/leaf core and then be coated in transparents to make them into rounds (clear, med blue and amethyst). I have tried every way that I can think of to prevent the silver core from fuming the outside glass and getting that insidious gold tarnish. I have reduced it before applying the top colour, I have worked the glass as cool as I can - which works partially when you start to lay the top colour on until you then try and melt it into a round (no matter how slow I went). I am getting really narked off with this. As the beads are so small (smallest size on a cg beadroller) I can't get enough distance between the flame and heat of the outer of the bead and the inside thus resulting in considerable and consistent fuming.

Harumpfh.

Can anyone proffer any other suggestions please.

Many thanks

Steampunkglass

I've not tried it myself, but have you tried paladium leaf instead, it looks silver.  ???

Lush!



www.lushlampwork.etsy.com

AnnaSpanna


Lush!



www.lushlampwork.etsy.com

Trudi

Hmm I think Glen has a good poiint - it will also not burn off or break up as much as silver will with to much heat!

Anna - I have some if you want to try it before I send off the cab mandrel!

AnnaSpanna



Magpie

It might be tricky keeping them small, but could you try encasing them in a thin layer of clear before using the top colour, then the silver and top colour of glass won't actually come into contact with each other.

julieHB

I might be totally dumb here, but when you fully encase the core there shouldn't be any fuming..... I know certain clears reacts with the silver foil and looks gold instead of silver - instead of clear you can use a very, very light blue/aqua to keep the silver looking silver and not gold. I'm a little at a l;oss why amethyst and blue doesn't stay true, though.

Are you burning in the silver foil before encasing, or are you making foil beads?

Another way to ensure there is no fuming is to not let the foil go completely to the end of the initial barrel, so you are absolutely sure there is no silver left to fume after encasing.

Sorry if I have completely misunderstood and haven't been of any help at all!!!
Julie xx

                           My Webbie - My Flickr

Redhotsal

#10
If you are using CIM to cover the silver that's probably your problem. If you try it with Effetre it should be okay.

AnnaSpanna

no def using effetre and basically whenever the glass directly over the silver gets hot it just fumes and goes gold (am making foil beads and so am not wanting to burn it in before I encase). I have had the most success with working the amethyst very cool and not getting quite so much fuming but then inevitably when I go for the final shape the core gets very hot very quickly as it is so close to the outer edge and bam - the whole lot goes patchy gold/fumed. Very frustrating. Am going to try some paladium and see how I get on with that. But thank you for all your advice so far  ;D

JaySpangles

See DragonJools Blog Saturday, October 24, 2009 for item about silver foil and encasing.  Just a bit of extra info to add to your memory bank.
http://dragonjools.blogspot.com/2009_10_01_archive.html

turnedlight

I was trying to do it with amber glass over silver recently, and I have decided to tell the person I can't do it, because it just went a horrible dirty grey. I have had trouble with silver wire going gold, effetre 006 is best to stop this and have the flame slightly reducing but not smokey or the clear will go dirty. I like the sound of the palladium, if it works let me know!
I was looking at murano beads recently and they were listed as gold leaf, or white gold leaf, and it got me wondering - is the seller mistaken or is that what they use?
kathryn

Lush!

It does look gold on the marver, but definitely looks silver on the bead - what do you think?

http://www.youtube.com/watch?v=EMn9H0b85To&feature=related


www.lushlampwork.etsy.com