Plowden and Thompson: Difference between revisions
New page: Plowden and Thompson are specialist glass manufacturers and coloured glass suppliers for studio and beadmaking, they also manufacture for industrial, medical, commercial and recrea... |
Added colours and working notes |
||
| (One intermediate revision by one other user not shown) | |||
| Line 2: | Line 2: | ||
Based in Stourbridge in the West Midlands they have been producing glass since 1922. | Based in Stourbridge in the West Midlands they have been producing glass since 1922. | ||
For the studio artist and [[ | For the studio artist and [[lampworker]] they produce two different ranges of [[soft glass]] either with a [[CoE]] of 93 or 100 in a variety of colours both [[opaque]] and [[transparent]]. | ||
Rods sizes are available in diameters 5-7mm 6-8mm,7-9mm,8-10mm and 10-12mm | Rods sizes are available in diameters 5-7mm 6-8mm,7-9mm,8-10mm and 10-12mm | ||
They also supply [[powders]] and [[chips]] of the same [[glass]] | They also supply [[powders]] and [[chips]] of the same [[glass]]. | ||
Plowden and Thompson were also very influential in the introduction of [[glass bead making]] into the UK. | Plowden and Thompson were also very influential in the introduction of [[glass bead making]] into the UK. | ||
They also stock Glass Alchemy [[borosilicate]] and [[Reichenbach]] 96 CoE glass. | |||
== CoE 100 Colours == | |||
The information below is a combination of Plowden & Thompson's working notes in their 2009 catalogue, and testing done by members of Frit-Happens! Generally speaking, these colours are noticeably stiffer than 104 CoE, particularly the transparent blues and greens. | |||
Manufacturer's notes: For best results these rods should be heated in a gentle oxygen rich flame - about 3 inches away from the torch. All the colours work very well with each other even if the consistency is different. | |||
=== Transparent === | |||
{| class="wikitable sortable" width=90% | |||
|- | |||
! width=50px|Stock Number | |||
! Colour | |||
! Properties | |||
! Comments | |||
|- | |||
|401 | |||
|Clear x7 | |||
|Very soft | |||
| | |||
|- | |||
|403 | |||
|Golden Yellow | |||
|Light-med amber | |||
| | |||
|- | |||
|404 | |||
|Citrus Yellow | |||
| | |||
| | |||
|- | |||
|405 | |||
|Amber | |||
| | |||
|Use a very gentle flame - does not like being overheated | |||
|- | |||
|406 | |||
|Light Orange | |||
| | |||
| | |||
|- | |||
|407 | |||
|Clear Red | |||
|Available as powder/chip only | |||
| | |||
|- | |||
|408 | |||
|Flame Red | |||
|Available as powder/chip only | |||
| | |||
|- | |||
|409 | |||
|Ruby | |||
|Ambery red, 'difficult' | |||
|Use a low Oxy flame. Can lose all the colour if overheated. Can bubble and burn. OK in a very gentle flame. Can turn an amber colour. | |||
|- | |||
|410 | |||
|Nile Green | |||
|Rich emerald green | |||
|Use a very gentle flame - does not like being overheated | |||
|- | |||
|411 | |||
|Mid Green | |||
|Rich green | |||
| | |||
|- | |||
|412 | |||
|Emerald Green | |||
|Rich green, 'difficult' | |||
|Slightly stiff and bubbles - mid green is MUCH better | |||
|- | |||
|413 | |||
|Antique Green | |||
|Dark green | |||
|Very dark as a self-coloured spacer. Boils, but less than the blues. | |||
|- | |||
|414 | |||
|Holly Green | |||
| | |||
| | |||
|- | |||
|415 | |||
|Daylight Blue | |||
|Transparent turquoise | |||
|Boils easily. | |||
|- | |||
|416 | |||
|Pacific Blue | |||
| | |||
| | |||
|- | |||
|417 | |||
|Sky Blue | |||
|Available as powder/chip only | |||
| | |||
|- | |||
|418 | |||
|Light Blue | |||
|Rich blue, not too light | |||
|Use a very gentle flame - does not like being overheated | |||
|- | |||
|419 | |||
|Electric Blue | |||
|Rich turquoise blue, stiff | |||
|Likes a cool flame. Boils very easily. | |||
|- | |||
|420 | |||
|Royal Blue | |||
|Cobalt blue | |||
| | |||
|- | |||
|421 | |||
|Midnight Blue | |||
|Available as powder/chip only | |||
| | |||
|- | |||
|422 | |||
|Mauve | |||
|Amethyst | |||
|Use a very gentle flame - does not like being overheated | |||
|- | |||
|423 | |||
|Violet | |||
| | |||
| | |||
|- | |||
|424 | |||
|Purple | |||
| | |||
| | |||
|- | |||
|425 | |||
|Smoke | |||
|Very pale grey | |||
| | |||
|- | |||
|427 | |||
|Gold Pink | |||
|Very pale pink | |||
|Can go clear if worked too long. Very pretty over a white core | |||
|- | |||
|429 | |||
|Rose Pink | |||
|Very pale pink | |||
|Almost clear | |||
|- | |||
|430 | |||
|Pink | |||
| | |||
| | |||
|- | |||
|431 | |||
|Cherry | |||
| | |||
| | |||
|- | |||
|432 | |||
|Garnet | |||
| | |||
| | |||
|- | |||
|434 | |||
|British Green | |||
| | |||
| | |||
|- | |||
|435 | |||
|Dark Amber | |||
| | |||
|Very dark on its own, looks good over white | |||
|- | |||
|436 | |||
|Florida Blue | |||
| | |||
| | |||
|- | |||
| | |||
|Cider | |||
|Very light amber | |||
| | |||
|- | |||
| | |||
|Gold Ruby | |||
|Rich deep pink | |||
|Can go clear, allow to cool and then strike in the flame to bring back the rich colour. | |||
|- | |||
| | |||
|Light Amber Eyeshell | |||
|Light amber | |||
| | |||
|- | |||
| | |||
|Mandarin | |||
| | |||
| | |||
|- | |||
| | |||
|Satsuma | |||
| | |||
| | |||
|- | |||
| | |||
|Water Green | |||
|Watery green | |||
| | |||
|- | |||
|600 | |||
|Soft Clear | |||
|Soft casing cane | |||
| | |||
|- | |||
|601 | |||
|Soft Ruby | |||
|Soft casing cane | |||
| | |||
|- | |||
|} | |||
=== Opaque (and Misty) === | |||
{| class="wikitable sortable" width=90% | |||
|- | |||
! width=50px|Stock Number | |||
! Colour | |||
! Properties | |||
! Comments | |||
|- | |||
|501 | |||
|Pearl White | |||
|Transparent & Opaque! | |||
|Looks transparent with a very slight purple tint. Turns pearl white when left to cool and then 'kissed' with a oxy reduced flame, otherwise it remains transparent. Got a slight fizz to it. | |||
|- | |||
|502 | |||
|Diopal White | |||
|Slightly translucent, soft. | |||
|Does not yellow with fine silver. | |||
|- | |||
|503 | |||
|Canary Yellow | |||
|Acid yellow | |||
|Stays semi-translucent, streaky. Ringed rod. | |||
|- | |||
|504 | |||
|Egg Yellow | |||
| | |||
| | |||
|- | |||
|505 | |||
|Daffodil Yellow | |||
| | |||
|Bubbles and pits - use in a very very cool flame and it is OK. | |||
|- | |||
|506 | |||
|Bright Orange | |||
|'Difficult' | |||
|Bubbles and pits, burnt brown specks easily. May not be visible until cooled. Ringed rod. | |||
|- | |||
|507 | |||
|Post Office Red | |||
|Rich red | |||
| | |||
|- | |||
|508 | |||
|Pastel Green | |||
|Available as powder/chip only | |||
| | |||
|- | |||
|511 | |||
|Birch Green | |||
|Sage/teal green | |||
|Streaky. | |||
|- | |||
|512 | |||
|Turquoise | |||
|Light baby blue | |||
|This looks almost encased in the rod form but when heated has a slight pearly look to it. Needs an Oxy rich flame. | |||
|- | |||
|513 | |||
|Monsoon Blue | |||
|Turquoise | |||
| | |||
|- | |||
|514 | |||
|Cobalt Opal Blue | |||
|Rich bright blue, med-soft. | |||
| | |||
|- | |||
|515 | |||
|Navy Blue | |||
|Available as powder/chip only | |||
| | |||
|- | |||
|517 | |||
|Grey | |||
| | |||
| | |||
|- | |||
|518 | |||
|Black | |||
|Black/silver | |||
|Likes a cool oxy reduced flame. If the flame is too hot can bubble and pit. Turns silver with little effort. Can be burned off and brought to surface again for darker result with hints of bronze. Black outline when other colours used on top. Returns to black under encasement. | |||
|- | |||
|519 | |||
|Mint Green | |||
|Medium minty green | |||
|Rough, flaky 'cellophane' surface after cooling. (May be user error!) Reaction line with reds, oranges, yellows. | |||
|- | |||
|520 | |||
|Tangerine | |||
| | |||
| | |||
|- | |||
|521 | |||
|Primrose | |||
| | |||
| | |||
|- | |||
|522 | |||
|Plum | |||
|Deep red | |||
|Very well behaved red | |||
|- | |||
|523 | |||
|Lavender | |||
| | |||
| | |||
|- | |||
|524 | |||
|Dark Post Office Red | |||
|Dark crimson | |||
| | |||
|- | |||
| | |||
|Burnt Orange | |||
|Yellow-orange satsuma | |||
|Streaky. Ringed rod. | |||
|- | |||
| | |||
|Misty Orange | |||
|Translucent streaky orange | |||
|Easy to use, very nice colour. Rod very obviously ringed. | |||
|- | |||
| | |||
|NT Green | |||
|Light green | |||
| | |||
|- | |||
| | |||
|Pearl Violet | |||
| | |||
| | |||
|- | |||
| | |||
|Post Office Orange | |||
|Reddish orange | |||
|May have slight streakiness. Ringed rod. | |||
|- | |||
| | |||
|Vanilla | |||
|Light browny cream, soft | |||
|An ivory, darker and warmer in tone than Effetre dark ivory. Less reactive. Haven't seen a 104 colour like it! | |||
|- | |||
|} | |||
== CoE 93 Colours == | |||
The information below is taken from Plowden & Thompson's working notes in their 2009 catalogue. | |||
Manufacturer's notes: For best results these rods should be heated in a gentle oxygen rich flame - about 3 inches away from the torch. All the colours work very well with each other even if the consistency is different. The pale transparent such as Salmon and Parisian Blue encased over opal pink and heather produces rich amethyst shades. Fire Engine Red and the Yellows should be thoroughly tested before using with other colours to avoid disappointment. The clear rods are very easy to use and encase all the colours very well and work well with the range of Dichroic sheet glass also available. | |||
=== Transparent === | |||
{| class="wikitable sortable" width=90% | |||
|- | |||
! width=50px|Stock Number | |||
! Colour | |||
! Properties | |||
! Comments | |||
|- | |||
|800 | |||
|Clear | |||
|Crystal clear | |||
|A great crystal clear glass - great for encasing with a creamy texture. Very easy to control. The rod must be spotlessly clean before using. Can produce a slight fizz if overheated. Suitable for encasing over the P & T range of Dichroic Glass | |||
|- | |||
|801 | |||
|Neon Blue | |||
|Dark cobalt blue, stiff | |||
|Not suitable for encasing - too dark. Makes great stringers for use on pale glass | |||
|- | |||
|802 | |||
|Neon Green | |||
|Dark bottle green, stiff | |||
|Not suitable for encasing - too dark. Makes great stringers for use on pale glass. | |||
|- | |||
|803 | |||
|Parisian Blue | |||
|Pale baby blue, soft | |||
|Looks great if encased over white, opal pink or heather. Will turn an attractive pale grey in an oxygen reduce flame. | |||
|- | |||
|804 | |||
|Atlantic Blue | |||
|Very pale grey/blue, very soft | |||
|Can produce attractive tiny fizzy bubbles in an oxygen rich flame. If you don't want the bubbles use a very gentle flame. Very pretty subtle colour. | |||
|- | |||
|805 | |||
|Dusky Pink | |||
| | |||
| | |||
|- | |||
|806 | |||
|Pink | |||
| | |||
| | |||
|- | |||
|810 | |||
|Ice Pink | |||
| | |||
| | |||
|- | |||
|812 | |||
|Suffolk Green | |||
|Soft | |||
|Colour is not affected by an oxygen reduced flame. | |||
|- | |||
|813 | |||
|Neon Ruby | |||
| | |||
| | |||
|- | |||
|817 | |||
|Rose Pink | |||
|Very pale pink | |||
|A very subtle pink - could be useful for encasing | |||
|- | |||
| | |||
|Elephant | |||
| | |||
| | |||
|- | |||
| | |||
|Miami Blue | |||
| | |||
| | |||
|- | |||
| | |||
|Neon Yellow | |||
| | |||
| | |||
|- | |||
| | |||
|Salmon | |||
|Pale pink | |||
|Looks great if encased over white, opal pink or heather. | |||
|- | |||
| | |||
|Soft Ruby | |||
|Dark transparent red, difficult | |||
|Can turn clear. | |||
|- | |||
|} | |||
=== Opaque (and Misty) === | |||
{| class="wikitable sortable" width=90% | |||
|- | |||
! width=50px|Stock Number | |||
! Colour | |||
! Properties | |||
! Comments | |||
|- | |||
|902 | |||
|Banana | |||
|Semi-transparent yellow, med stiff. Difficult. | |||
|Bubbles and pits if not used in a very gentle frame. Work at tip of an oxygen rich flame. Can go clear if too hot and overworked | |||
|- | |||
|903 | |||
|Sherbet | |||
| | |||
| | |||
|- | |||
|904 | |||
|Pillar Box Red | |||
|Crimson | |||
|Use in a cool flame - bubbles if too hot. Can turn to transparent red or to almost clear. | |||
|- | |||
|905 | |||
|Fire Engine Red | |||
|Dark red, stiff, difficult | |||
|Use an Oxygen Rich flame - keep at the end of the flame a nice colour once you get use to it. Don't over work. | |||
|- | |||
|906 | |||
|Candy Pink | |||
|Pale baby pink, soft | |||
|Goes almost clear when heated - colour returns when cool. | |||
|- | |||
|907 | |||
|Gold Opal Pink | |||
|Deep pink | |||
|Can go patchy if overheated. Stringers can appear transparent when pulled, but turns back to opaque when used. | |||
|- | |||
|908 | |||
|Heather | |||
|Deep lavender blue | |||
|A lovely glass to work with. | |||
|- | |||
|909 | |||
|Bluebell | |||
|Deep bluebell blue | |||
|Lovely and easy to work with - slightly streaky - can look like Lapis Lazuli. Very good with white but the colour can be patchy if use close to other colours. | |||
|- | |||
|910 | |||
|Apple Green | |||
|Crisp med green, soft | |||
|Stringers can go transparent - very attractive colour. | |||
|- | |||
|911 | |||
|Jade Green | |||
|Pale jade | |||
|Very easy to use and a lovely colour. Can go murky in an oxygen reduced flame. | |||
|- | |||
|912 | |||
|Forest Green | |||
|Darkish green | |||
|Very easy to use and a lovely colour. | |||
|- | |||
|913 | |||
|Typhoon | |||
|Rich turquoise blue | |||
|Use an oxygen rich flame - will turn orange and streaky in a reduced oxygen flame. Great colour. | |||
|- | |||
|914 | |||
|Jet Black | |||
|Black | |||
|A wonderful jet black glass - very well behaved! | |||
|- | |||
|915 | |||
|Arctic White | |||
|Snow white, soft | |||
|Goes clear when heated, soon cools back down to a pure white - very useful - works well with ALL other colours in the range. | |||
|- | |||
|916 | |||
|Mango | |||
|Rich vivid orange, med stiff | |||
|Can bubble if too hot - great colour. | |||
|- | |||
| | |||
|Caramel | |||
| | |||
| | |||
|- | |||
| | |||
|Cream | |||
| | |||
| | |||
|- | |||
| | |||
|Pistachio | |||
| | |||
| | |||
|- | |||
| | |||
|Powder Blue | |||
| | |||
| | |||
|- | |||
| | |||
|Tangerine | |||
|Vibrant orange | |||
|Work in a cool flame. Can boil if too hot but does not pit. Stringers can go transparent but returns to normal when used. Nice colour not too vivid. | |||
|- | |||
| | |||
|Toffee | |||
| | |||
| | |||
|- | |||
| | |||
|Yellow Total | |||
|Sunshine yellow, med/difficult | |||
|Bubbles and pits if not used in a very gentle frame. Work at tip of an oxygen rich flame. Use in small quantities - not suitable for large areas of colour. Looks good encased in clear or with Bluebell. | |||
|- | |||
|} | |||
== Further information == | == Further information == | ||
For further information see [http://www.plowden-thompson.com/ The Manufacturers Website] | For further information see [http://www.plowden-thompson.com/ The Manufacturers Website] | ||
<!-- Please leave this at the bottom --> | |||
[[Category:Types of Glass]] | |||
Latest revision as of 14:36, 19 July 2010
Plowden and Thompson are specialist glass manufacturers and coloured glass suppliers for studio and beadmaking, they also manufacture for industrial, medical, commercial and recreational uses. Based in Stourbridge in the West Midlands they have been producing glass since 1922.
For the studio artist and lampworker they produce two different ranges of soft glass either with a CoE of 93 or 100 in a variety of colours both opaque and transparent.
Rods sizes are available in diameters 5-7mm 6-8mm,7-9mm,8-10mm and 10-12mm They also supply powders and chips of the same glass.
Plowden and Thompson were also very influential in the introduction of glass bead making into the UK.
They also stock Glass Alchemy borosilicate and Reichenbach 96 CoE glass.
CoE 100 Colours
The information below is a combination of Plowden & Thompson's working notes in their 2009 catalogue, and testing done by members of Frit-Happens! Generally speaking, these colours are noticeably stiffer than 104 CoE, particularly the transparent blues and greens.
Manufacturer's notes: For best results these rods should be heated in a gentle oxygen rich flame - about 3 inches away from the torch. All the colours work very well with each other even if the consistency is different.
Transparent
| Stock Number | Colour | Properties | Comments |
|---|---|---|---|
| 401 | Clear x7 | Very soft | |
| 403 | Golden Yellow | Light-med amber | |
| 404 | Citrus Yellow | ||
| 405 | Amber | Use a very gentle flame - does not like being overheated | |
| 406 | Light Orange | ||
| 407 | Clear Red | Available as powder/chip only | |
| 408 | Flame Red | Available as powder/chip only | |
| 409 | Ruby | Ambery red, 'difficult' | Use a low Oxy flame. Can lose all the colour if overheated. Can bubble and burn. OK in a very gentle flame. Can turn an amber colour. |
| 410 | Nile Green | Rich emerald green | Use a very gentle flame - does not like being overheated |
| 411 | Mid Green | Rich green | |
| 412 | Emerald Green | Rich green, 'difficult' | Slightly stiff and bubbles - mid green is MUCH better |
| 413 | Antique Green | Dark green | Very dark as a self-coloured spacer. Boils, but less than the blues. |
| 414 | Holly Green | ||
| 415 | Daylight Blue | Transparent turquoise | Boils easily. |
| 416 | Pacific Blue | ||
| 417 | Sky Blue | Available as powder/chip only | |
| 418 | Light Blue | Rich blue, not too light | Use a very gentle flame - does not like being overheated |
| 419 | Electric Blue | Rich turquoise blue, stiff | Likes a cool flame. Boils very easily. |
| 420 | Royal Blue | Cobalt blue | |
| 421 | Midnight Blue | Available as powder/chip only | |
| 422 | Mauve | Amethyst | Use a very gentle flame - does not like being overheated |
| 423 | Violet | ||
| 424 | Purple | ||
| 425 | Smoke | Very pale grey | |
| 427 | Gold Pink | Very pale pink | Can go clear if worked too long. Very pretty over a white core |
| 429 | Rose Pink | Very pale pink | Almost clear |
| 430 | Pink | ||
| 431 | Cherry | ||
| 432 | Garnet | ||
| 434 | British Green | ||
| 435 | Dark Amber | Very dark on its own, looks good over white | |
| 436 | Florida Blue | ||
| Cider | Very light amber | ||
| Gold Ruby | Rich deep pink | Can go clear, allow to cool and then strike in the flame to bring back the rich colour. | |
| Light Amber Eyeshell | Light amber | ||
| Mandarin | |||
| Satsuma | |||
| Water Green | Watery green | ||
| 600 | Soft Clear | Soft casing cane | |
| 601 | Soft Ruby | Soft casing cane |
Opaque (and Misty)
| Stock Number | Colour | Properties | Comments |
|---|---|---|---|
| 501 | Pearl White | Transparent & Opaque! | Looks transparent with a very slight purple tint. Turns pearl white when left to cool and then 'kissed' with a oxy reduced flame, otherwise it remains transparent. Got a slight fizz to it. |
| 502 | Diopal White | Slightly translucent, soft. | Does not yellow with fine silver. |
| 503 | Canary Yellow | Acid yellow | Stays semi-translucent, streaky. Ringed rod. |
| 504 | Egg Yellow | ||
| 505 | Daffodil Yellow | Bubbles and pits - use in a very very cool flame and it is OK. | |
| 506 | Bright Orange | 'Difficult' | Bubbles and pits, burnt brown specks easily. May not be visible until cooled. Ringed rod. |
| 507 | Post Office Red | Rich red | |
| 508 | Pastel Green | Available as powder/chip only | |
| 511 | Birch Green | Sage/teal green | Streaky. |
| 512 | Turquoise | Light baby blue | This looks almost encased in the rod form but when heated has a slight pearly look to it. Needs an Oxy rich flame. |
| 513 | Monsoon Blue | Turquoise | |
| 514 | Cobalt Opal Blue | Rich bright blue, med-soft. | |
| 515 | Navy Blue | Available as powder/chip only | |
| 517 | Grey | ||
| 518 | Black | Black/silver | Likes a cool oxy reduced flame. If the flame is too hot can bubble and pit. Turns silver with little effort. Can be burned off and brought to surface again for darker result with hints of bronze. Black outline when other colours used on top. Returns to black under encasement. |
| 519 | Mint Green | Medium minty green | Rough, flaky 'cellophane' surface after cooling. (May be user error!) Reaction line with reds, oranges, yellows. |
| 520 | Tangerine | ||
| 521 | Primrose | ||
| 522 | Plum | Deep red | Very well behaved red |
| 523 | Lavender | ||
| 524 | Dark Post Office Red | Dark crimson | |
| Burnt Orange | Yellow-orange satsuma | Streaky. Ringed rod. | |
| Misty Orange | Translucent streaky orange | Easy to use, very nice colour. Rod very obviously ringed. | |
| NT Green | Light green | ||
| Pearl Violet | |||
| Post Office Orange | Reddish orange | May have slight streakiness. Ringed rod. | |
| Vanilla | Light browny cream, soft | An ivory, darker and warmer in tone than Effetre dark ivory. Less reactive. Haven't seen a 104 colour like it! |
CoE 93 Colours
The information below is taken from Plowden & Thompson's working notes in their 2009 catalogue.
Manufacturer's notes: For best results these rods should be heated in a gentle oxygen rich flame - about 3 inches away from the torch. All the colours work very well with each other even if the consistency is different. The pale transparent such as Salmon and Parisian Blue encased over opal pink and heather produces rich amethyst shades. Fire Engine Red and the Yellows should be thoroughly tested before using with other colours to avoid disappointment. The clear rods are very easy to use and encase all the colours very well and work well with the range of Dichroic sheet glass also available.
Transparent
| Stock Number | Colour | Properties | Comments |
|---|---|---|---|
| 800 | Clear | Crystal clear | A great crystal clear glass - great for encasing with a creamy texture. Very easy to control. The rod must be spotlessly clean before using. Can produce a slight fizz if overheated. Suitable for encasing over the P & T range of Dichroic Glass |
| 801 | Neon Blue | Dark cobalt blue, stiff | Not suitable for encasing - too dark. Makes great stringers for use on pale glass |
| 802 | Neon Green | Dark bottle green, stiff | Not suitable for encasing - too dark. Makes great stringers for use on pale glass. |
| 803 | Parisian Blue | Pale baby blue, soft | Looks great if encased over white, opal pink or heather. Will turn an attractive pale grey in an oxygen reduce flame. |
| 804 | Atlantic Blue | Very pale grey/blue, very soft | Can produce attractive tiny fizzy bubbles in an oxygen rich flame. If you don't want the bubbles use a very gentle flame. Very pretty subtle colour. |
| 805 | Dusky Pink | ||
| 806 | Pink | ||
| 810 | Ice Pink | ||
| 812 | Suffolk Green | Soft | Colour is not affected by an oxygen reduced flame. |
| 813 | Neon Ruby | ||
| 817 | Rose Pink | Very pale pink | A very subtle pink - could be useful for encasing |
| Elephant | |||
| Miami Blue | |||
| Neon Yellow | |||
| Salmon | Pale pink | Looks great if encased over white, opal pink or heather. | |
| Soft Ruby | Dark transparent red, difficult | Can turn clear. |
Opaque (and Misty)
| Stock Number | Colour | Properties | Comments |
|---|---|---|---|
| 902 | Banana | Semi-transparent yellow, med stiff. Difficult. | Bubbles and pits if not used in a very gentle frame. Work at tip of an oxygen rich flame. Can go clear if too hot and overworked |
| 903 | Sherbet | ||
| 904 | Pillar Box Red | Crimson | Use in a cool flame - bubbles if too hot. Can turn to transparent red or to almost clear. |
| 905 | Fire Engine Red | Dark red, stiff, difficult | Use an Oxygen Rich flame - keep at the end of the flame a nice colour once you get use to it. Don't over work. |
| 906 | Candy Pink | Pale baby pink, soft | Goes almost clear when heated - colour returns when cool. |
| 907 | Gold Opal Pink | Deep pink | Can go patchy if overheated. Stringers can appear transparent when pulled, but turns back to opaque when used. |
| 908 | Heather | Deep lavender blue | A lovely glass to work with. |
| 909 | Bluebell | Deep bluebell blue | Lovely and easy to work with - slightly streaky - can look like Lapis Lazuli. Very good with white but the colour can be patchy if use close to other colours. |
| 910 | Apple Green | Crisp med green, soft | Stringers can go transparent - very attractive colour. |
| 911 | Jade Green | Pale jade | Very easy to use and a lovely colour. Can go murky in an oxygen reduced flame. |
| 912 | Forest Green | Darkish green | Very easy to use and a lovely colour. |
| 913 | Typhoon | Rich turquoise blue | Use an oxygen rich flame - will turn orange and streaky in a reduced oxygen flame. Great colour. |
| 914 | Jet Black | Black | A wonderful jet black glass - very well behaved! |
| 915 | Arctic White | Snow white, soft | Goes clear when heated, soon cools back down to a pure white - very useful - works well with ALL other colours in the range. |
| 916 | Mango | Rich vivid orange, med stiff | Can bubble if too hot - great colour. |
| Caramel | |||
| Cream | |||
| Pistachio | |||
| Powder Blue | |||
| Tangerine | Vibrant orange | Work in a cool flame. Can boil if too hot but does not pit. Stringers can go transparent but returns to normal when used. Nice colour not too vivid. | |
| Toffee | |||
| Yellow Total | Sunshine yellow, med/difficult | Bubbles and pits if not used in a very gentle frame. Work at tip of an oxygen rich flame. Use in small quantities - not suitable for large areas of colour. Looks good encased in clear or with Bluebell. |