6mm SLUMPING firing schedule (ARTISTA)
Post by:
handmadeheaven.biz
on
January 06, 2007, 04:59:50 PM
SLUMPING 6mm firing schedule ARTISTA
1. 175C/hr to
540C
0.10
2. AFAP or 9999C/hr to
700C
0.00
3. 100C/hr to
790C
0.00
4. AFAP or 9999C/hr to
560C
1.00
5. 66C/hr to
443C
0.00
6. 125C/hr to
393C
0.00
7. AFAP or 9999C/hr to
25C
0.00