Title: 6mm FULL FUSE firing schedule (ARTISTA)
Post by: handmadeheaven.biz on January 06, 2007, 10:46:37 AM
FULL FUSE 6mm firing schedule ARTISTA

1. 250C/hr to 540C   0.10

2. AFAP or 9999C/hr to 820C   0.12

3. AFAP or 9999C/hr to 560C   0.30

4. 66C/hr to 443C   0.00

5. 125C/hr to 393   0.00

6. AFAP or 9999C/hr to 25   0.00