Hello,
I have the bead release that came in a starter kit from Martin. More and more beads are now not coming off the mandrels. I have soaked them in water, put them in the freezer and always use pliers to hold the mandrel while twisting (or trying - causing blisters!!!!!) . What is the best bead release to use. My left hand is currently damaged after getting crushed at work and so the less pressure on my hand the better.
Ta
Chrissie
try molegrips on the mandrel - that's all i could use to get mine off
I never soak the beads and find that they just twist off when cool and the dry release crumbles away? If one gets a bit stuck I use rubber gloves and the big pliers but usually I can just twist them off with my hands.
Kaz
what bead release are you using as i have not had a bead yett in 4 years that i could just twist off by hand. I try first of all to twist the bead off dry using pliers to hold the mandrel. Some come off but this is getting less as time goes on. Is my bead release getting too old. :-\
possibly
i use foster fire and it simply crumbles away
I use fusion - bought a 3 pack from Martin
http://www.tuffnellglass.com/index.html?lmd=39511.559398
Kaz
I use fusion or smooth and tough for long or larger beads. I avoid the blue sludge at all costs, I found it a nightmare to try and get beads off.
fosterfire gets my vote :)
Quote from: Kaz on March 14, 2008, 10:26:56 PM
I use fusion - bought a 3 pack from Martin
http://www.tuffnellglass.com/index.html?lmd=39511.559398
Kaz
me too - no problems at all :)
I think you`ll find the bead release in the starter kit from Tuffnells is the Sludge. I spent yesterday reading through the forum trying to find the best bead release and have ordered some fosterfire from martin. My thumb can`t take anymore blisters. I read that the sludge needs to be "fresh" on the madrel and used within a day of being put on the mandrels otherwise it goes stale and wants to hold onto the beads. Looking forward to getting my little creations off the mandrels with ease! :D
I had the same problem with the blue sludge, as time went on it got harder and harder to get the beads off the mandrels, some are still permanantly stuck on them, I use Foster Fire now and its fab, just pull off the mandrels, no tools needed
I had the blue sludge and hated that, then I had the Fusion, this was ok but it was still a bugger to get beads of sometimes, easier to clean out the bead holes though, and dipping the mandrels was no problem.
Now I am on the foster fire, and I must say I love it for getting the beads off, just twist and go! :) its more of a bugger to clean out the holes though. I soak in warm soapy water and clean as usual then get a pipe cleaner thats been doubled over, and run that through. I don't like dipping with it, it runs, however much I try to thicken it up. So it takes me longer to dip but the pleasure of getting the beads off no problem is worth it :) :) :)
I've been getting the little pots from Martin from the start. They were blue, now they are beige (so I don't know what they are!) but they work fine.. the only thing I would say is sometimes the release breaks, but I guess you can't have it both ways?
Blue sludge is pants! I had no end of trouble with it >:(
I use Fusion at the moment, and have only had one stick, but I thought it would when I was making it as I had pulled the bead around too much and it had cracked the release! My advice is dump the sludge, and move on to something better - or you'll and up tearing your hair out ;) I've got a tub of Fosterfire I bought from Sooz waiting to be tried - but it seems that's getting good reports from beady pals, so no worries there!
I used superblue for years until changing to Fusion. Fusion is so much better. Blue will stick like the provervbial if you don't use it fresh. It's fine if you use it on the same day you dip it and if you have the layer thick enough but it's utter crap if it's "stale".
Thanks you've answered my problem brilliantly. I will put an order in asap. Some of my mandrels were dipped weeks ago which explains the problem. Thank you. ;D
I've got some of the blue and only use it on the tip of a mandrel if I'm pulling a twisty. I use the mandrel and pliers method and you can pretty much guarantee the release won't break when you pull!
Order some foster fire from sooz at ebay shop so now hopefully my problems will be over. :-*
Smooth and Tough is the best I've tried so far, pricey but the beads practically jump off the mandrels!
I've got Foster Fire at the moment and I'm still struggling to get the right consistency. Might go back to S&T next time.
I was surprised at how much water I've had to add. If I get it at about pancake mix consistency it works really well.
I've found as time goes on, my beads have been getting easier and easier to release. I used to have to use the pliers on at least half of a days batch, now it's only one of two - if that.
I have been putting this down to undoubtedly better technique as I become more proficient, I decided I must have been overheating less, taking less time to round out beads and the less time in the flame, the easier it is to release the beads and then I go and find that coating far in advance is a factor too!
I used to always dip a few days in advance and now I have fewer mandrels (due to some getting bent and permanently attached beads), I am now dipping the same day and flame drying the early ones (using Fusion), and after reading this thread realise that's probably why. This board really is a mine of information!
When mine get really difficult to release, I used to use a 50% solution of toilet duck in water soaked overnight, but I haven't had to resort to it in a while. Now when I get a tough one, I soak it in a half full sink of warmish water for half an hour, dry it all off and then dribble cold water either side of the bead for 5 seconds (no more) a side. The theory is that the bead is warmish and expanded and the cold water right next to the bead cools the mandrel which makes it shrink ever so slightly - it works for me - I haven't had to use the toilet duck solution for quite a while.
Fosterfire :D!
Otherwise the mole grips and rubber glove work a treat - but if it's really stuck, spray with WD40 and leave for a while.