Title: Gold stone gone funny green ?
Post by: the lady with the lamp on May 28, 2011, 01:35:48 PM
 ???Just got my nortel set up at last,so have been in my shed messing with my stuff tried to encase some goldstone but its gone a horrible green am i heating it too much thanks Parin.
Title: Re: Gold stone gone funny green ?
Post by: helenfc on May 28, 2011, 04:45:52 PM
Hi parin, goldstone goes green when it is in contact with silver. Were you using silver leaf or wire or silver glass in the beads? You want to try and work it quite cool, or the sparkle will burn out, but overheating shouldn't make it green. If you really want to use goldstone with silver, try making an encased goldstone stringer so they don't have to come into direct contact with each other.
Hope that helps x
Title: Re: Gold stone gone funny green ?
Post by: Jolene on May 28, 2011, 06:18:26 PM
Well I didn't know that! ;D
Title: Re: Gold stone gone funny green ?
Post by: Kaz on May 28, 2011, 06:28:00 PM
Me neither ;D
Title: Re: Gold stone gone funny green ?
Post by: Jolene on May 28, 2011, 06:36:20 PM
Is it in any way any sort of attractive shade of green? lol
Title: Re: Gold stone gone funny green ?
Post by: helenfc on May 28, 2011, 07:01:35 PM
I think so, it kind of looks like verdigris (sp?) Copper. Effetre black rolled in silver leaf then on golstone frit is quite cool! X
Title: Re: Gold stone gone funny green ?
Post by: Redhotsal on May 28, 2011, 09:20:33 PM
It has probably gone green because you have may have heated it very strongly and with an oxygen rich flame? Try going slower and having the flame slightly reducing - a little more propane and slightly bushy on the candles. 
You may not have had this trouble before on the hothead as that is a slightly reducing flame anyway.
Title: Re: Gold stone gone funny green ?
Post by: Trudi on May 28, 2011, 09:28:06 PM
Quote from: helenfc on May 28, 2011, 04:45:52 PM
Hi parin, goldstone goes green when it is in contact with silver. Were you using silver leaf or wire or silver glass in the beads? You want to try and work it quite cool, or the sparkle will burn out, but overheating shouldn't make it green. If you really want to use goldstone with silver, try making an encased goldstone stringer so they don't have to come into direct contact with each other.
Hope that helps x

Well I never!
Title: Re: Gold stone gone funny green ?
Post by: the lady with the lamp on May 29, 2011, 05:17:24 PM
 ;DThanks will try that Parin.
Title: Re: Gold stone gone funny green ?
Post by: SueP on May 29, 2011, 05:37:57 PM
hi

This is what it does with silver leaf - love it ;D

(http://i324.photobucket.com/albums/k329/Blueflamebeads_photos/April%20Beads%202011/copper.jpg)
Title: Re: Gold stone gone funny green ?
Post by: Dee Dee on May 30, 2011, 12:58:52 AM
They're fab, Sue, great reaction! ;D