Lampwork => Common Problems => Topic started by: noora on April 27, 2011, 05:05:24 PM

Title: Cabochon mandrels, how hot?
Post by: noora on April 27, 2011, 05:05:24 PM
Today I had a play with my pair of new cabochon mandrels. First one turned out okay, second one popped off while I was applying a glass. If I understand this correctly it may be because the mandrel got too cold. So how hot should the mandrel be? I heat up normal mandrels until they glow a bit before I start, but heating up the big disc on the cab mandrel until it glows seems like it would take ages on my Minor so I didn't do that. Should I have heated it up until it glows anyway?

Title: Re: Cabochon mandrels, how hot?
Post by: MangoBeads on April 27, 2011, 05:14:42 PM
What popped off Noora the bead or the bead release ? you should treat in the same way as a mandrel and heat up before applying glass . Sometimes i find the bead release pops off the edges but that dosnt cause a problem . The bead release may also be too thick - give the mandrel a good fast spin when you dip it to get an even coating. Hope that helps x
Title: Re: Cabochon mandrels, how hot?
Post by: noora on April 27, 2011, 05:31:41 PM
Thanks Manda :-) It was the glass that popped off, the bead release seems intact except for the bit on the top of the "knob" which was left inside the cab. I did heat the disc a bit, but not until it glowed and probably way too little. I'll try more heat next time then, I guess I was too impatient to try the new mandrels (and the new glass and the new frit... too much new stuff at once!) :-)

My bead release is quite thin at the moment, I managed to water it a bit too much last time it had turned goopy...
Title: Re: Cabochon mandrels, how hot?
Post by: MangoBeads on April 27, 2011, 06:01:53 PM
Does sound as though the whole thing was a bit on the cool side then  :) its so exciting with lots of new toys to play with !!! I can feel your excitement !