Frit-Happens !

Lampwork => Common Problems => Topic started by: beadammed on April 21, 2011, 07:46:53 PM

Title: reducing
Post by: beadammed on April 21, 2011, 07:46:53 PM
Hi folks, I've mentioned my lack of ability to get anything out of reduction glass (except a mirror effect on triton) but I've just been in the shed to have another go and now have enough sludge to build a wall.   :'(
I've tried turning gas up and oxy down....nowt.  I put the bead just above the tip of the yellow (looking at FH logo).  People mention wafting it in and out but I tend to keep it in a couple of seconds as otherwise nothing happens.  Any last suggestions before it all goes in the bin?
Also what does magic and multicolour do other than grey and brown?   :'( :'( :'(
(Not my best beading day)
Title: Re: reducing
Post by: helbels on April 21, 2011, 07:53:28 PM
What torch are you on? And can you take a picture of your flame both "normally" and when reducing?

It might help us to help you x
Title: Re: reducing
Post by: beadammed on April 21, 2011, 08:17:32 PM
Now that's a good idea Helen ;D.  I'll get my sister to take a photo this weekend.  I'm getting photos taken to apply for SRA so I'll see if I can get some of the flame and post it.  Thanks for that.  Watch this space..........
Title: Re: reducing
Post by: awrylemming on April 21, 2011, 08:19:16 PM
Don't lose heart - plenty of us have produced material for the foundations, when the breakthrough comes, it'll be worthwhile, I promise x
Title: Re: reducing
Post by: flowerjasper on April 21, 2011, 08:35:03 PM
its so frustrating when a technique or glass eludes you,
dont give up  ;)
do you have hades? if so make a twistie with hades and magic, a small bead of dirty martini, wrap the twistie round the small bead, melt in, you can really let it get hot and swirl round the bead, then encase in 006.... magic!
as helen says pictures may help,
sandy
Title: Re: reducing
Post by: Alison G on April 21, 2011, 09:14:21 PM
Quote from: awrylemming on April 21, 2011, 08:19:16 PM
Don't lose heart - plenty of us have produced material for the foundations, when the breakthrough comes, it'll be worthwhile, I promise x

Sue is right. We've all done it and even now I can't get Elektra or Gaia to behave. I found really letting the bead cool before you even and try and reduce works best. And take it straight out if it glows, just a real dance in the flame. I'm an oxy down girl but I know some people prefer propane up.

Keep going! It's a pity it's so expensive, I know.

Never tried Magic but I love Multi in both types, I strike rather than reduce those though.
Title: Re: reducing
Post by: helenfc on April 21, 2011, 09:26:04 PM
what glass are you struggling to reduce? It does really help if, as Alison says, the bead is cooled down so the glow is pretty much gone. You should see it go almost mirror shiny in the flame. Try this with Magic if you cant make it strike, its goes a lovely bronze when reduced! Good Luck! xx
Title: Re: reducing
Post by: stuwaudby on April 21, 2011, 09:46:58 PM
Reichenbach magic and multicolour take a bit of getting used to, it took me ages to get anything. Take a look at http://www.runnyglass.com/page3.htm (http://www.runnyglass.com/page3.htm) and look for the Magic necklace for an example of what can be done. Those beads are made from a mix of multi and vetrofond clear.

For starters avoid reducing it unless you want a metallic surface over green brown sludge. Keep it worked in neutral to oxidising. When done take the bead well out of the flame and wait about 45 seconds (longer for large beads). The glow should have just about gone. Introduce it to the back of the flame to strike, all you will get is dirty yellow colours. If I repeat strike then I can sometimes get some purples to appear. After all this the real magic happens in the kiln. Anneal at 512-520 for at least an hour to finish the strike crossed fingers required. Results can be random, even between the same beads on the same mandrel. I have had beautiful purples on one bead a smudgy yellow on the other!

I have never had any success using magic / multi on the surface, it always goes opaque green brown. It has to be encased. I find multi gives easier results than magic.

Try making a cane using black base with a couple of stripes of multi. Give it a lot of twists as you pull it to about 5mm. A couple of wraps of this cane followed by a couple of wraps of clear to encase will give an almost boro like bead.

Title: Re: reducing
Post by: beadammed on April 21, 2011, 10:00:07 PM
WOW Stuart, that really is magic.  I'm going to try out your suggestions particularly leaving it to kiln strike. I have a lot of magic as I got some as a gift so I'd really like to get it working.  I love the effect you got.  I'll try the twisty too.
I'm all fired up now.  I can see my uni assignment being put off again! Still... it's all in the name of science!
Title: Re: reducing
Post by: beadammed on April 21, 2011, 10:02:12 PM
4got to ask...Do you strike before or after encasing?
Title: Re: reducing
Post by: awrylemming on April 21, 2011, 10:56:30 PM
I have to say, I have some lovely beads with Multi on the surface - wonderful purples, blues and greens, but it takes a fair while to get the colours.  I repeatedly strike and rapidly cool on brass, don't seem to achieve the same colours from slow, natural cooling.  Haven't tried encasing yet, I think I may have a go at that now ...
Title: Re: reducing
Post by: Blue Box Studio on April 21, 2011, 11:02:44 PM
Can't do a thing with multi, but mine's plain multi not dark multi.  Didn't get anywhere with DH glass until I bought a tut off Ebay.  Murphy then took a hand and gave me colours!  I've still not got the tut into the shedio or read it, it just took the idle threat of 'if you don't work this time I'm getting a tut'.  My June project is to read the tutorials I've bought recently.

I have a customer who comes to a regular autumn fair and buys all my grotty green beads.  She loves the patterns and colours.  Haven't the heart to tell her they should be glorious purples and blues :(
Title: Re: reducing
Post by: awrylemming on April 22, 2011, 09:13:51 AM
Quote from: beadammed on April 21, 2011, 10:02:12 PM
4got to ask...Do you strike before or after encasing?

Sorry, missed this question.  You strike before encasing.  And I made an encased dark multi lentil last night, it's glorious, pinks, blues, purples etc, and I only struck it twice and briefly.  Thanks for that Stuwaudby  :)
Title: Re: reducing
Post by: beadammed on April 22, 2011, 10:06:28 AM
Thanks all! Off to my shed now all enthusiastic! Will also try to find customers that LURV Sludge colour (plasterers maybe).
p.s. If I get an 'F' for my structural genetics essay you are all to blame ;D
Title: Re: reducing
Post by: The Tartan Trout on April 27, 2011, 04:12:22 PM
Never fear...not just anybody can reduce expensive silver glass to varying shades of brown and green...it is a talent you know...welcome to my gang   :D :D :D
Title: Re: reducing
Post by: Donna@Rockin' Beads on April 27, 2011, 04:47:07 PM
Geraldine, I can certainly recommend an hour with Redhotsal to help unlock the mysteries of reducing and striking. I had an hour with her on Sunday and it helped HUGELY  ;D
She's a bit far from you though  :(
Maybe if you come down to visit me in my lovely Tavistock shop you can pop down to St Ives to see her  ;D ;D ;D
Good luck anyway  :)
Title: Re: reducing
Post by: beadammed on April 27, 2011, 10:01:49 PM
I managed down to Sal's course before so I should know the way.  I didn't have a great deal of luck with the reducing ergo: nae pictures.  I've decided once my masters is finished in September I'm hitting all the classes I can.  Head down till then tho!
Title: Re: reducing
Post by: stuwaudby on May 03, 2011, 12:58:51 PM
Quote from: awrylemming on April 22, 2011, 09:13:51 AM
Quote from: beadammed on April 21, 2011, 10:02:12 PM
4got to ask...Do you strike before or after encasing?

Sorry, missed this question.  You strike before encasing.  And I made an encased dark multi lentil last night, it's glorious, pinks, blues, purples etc, and I only struck it twice and briefly.  Thanks for that Stuwaudby  :)

Show us a picture!