Frit-Happens !

Lampwork => Common Problems => Topic started by: helbels on March 19, 2011, 09:31:20 PM

Title: At my wits end - overstriking
Post by: helbels on March 19, 2011, 09:31:20 PM
Hiya

My kiln (Bead Cube) hates Terranova.   I strike the Terranova in the flame, get it to the point where it's a nice streaky blue/purple, and pop the beads in the kiln.  What comes out the kiln at the other end is Murky Brown/Red beads.

I read that DH doesn't like a hot annealing temperature and so I turned my kiln down so I'm now annealing at 510.. but the beads are still coming out red/brown.  Multicolour Dark is coming out SO dark that it looks black.

Can I turn the kiln down yet further??  Will Effetre and CIM still anneal if I were to say, turn it down to 490?

I don't know what else to try  >:(
Title: Re: At my wits end - overstriking
Post by: Redhotsal on March 19, 2011, 09:43:38 PM
Your kiln may actually be hotter than the controller says it is. My Maxine runs hotter in real life that the controller says. For me it's not a problem - I just turn the temp down - one of my Maxines runs at "490" even though I'm pretty sure it is hotter than that. You can get the kiln calibrated - give Lee a call and ask him what he thinks. Alternatively you can just turn the kiln down. If it were me I would turn the kiln down until it was annealing your Terranova properly and then chuck in a couple of clear beads of CIM and Effetre. You can check them with a polariser to see whether they were actually annealing properly.
Title: Re: At my wits end - overstriking
Post by: helbels on March 19, 2011, 09:45:23 PM
Thanks Sal - will give it a go at 490 and see what happens.  It's so bloody annoying, its like witchcraft trying to conquer it's little ways!
Title: Re: At my wits end - overstriking
Post by: Redhotsal on March 19, 2011, 09:47:16 PM
All part of the fun and games...!  ;)
Title: Re: At my wits end - overstriking
Post by: julieHB on March 19, 2011, 10:39:35 PM
I'm going to repeat myself with posting a link to this blog: http://envisionsf.blogspot.com/2009/04/silver-glass-101-annealing-temperature.html

I really think the answer to your problem is to lower the temperature. But do it in stages, as explained in the blog. And, there is a difference between striking and reducing glasses. Have a read, and let's know what you think  :)
Title: Re: At my wits end - overstriking
Post by: Studio Girl on March 20, 2011, 09:15:40 AM
Just what I was going to say
pop a bit of charcoal in and see if that works

Margaret xx
Title: Re: At my wits end - overstriking
Post by: helbels on March 20, 2011, 09:19:45 AM
The charcoal isn't necessary - I have no problem with reduction glass, its the strikers that are giving me an issue.

I will turn the kiln down to 490 and give it another go.
Title: Re: At my wits end - overstriking
Post by: Pegasus on March 20, 2011, 02:06:35 PM
Helen, I lowered my kiln temp to 490c for this reason and it has made a vast improvement to my TN colours. Just another idea also, if you are striking the TN to blue-ish colour before putting it in the kiln, try stopping the striking before you get to this colour and pop in the kiln. For me I still find that the colour will develop (continue striking) in the kiln but only slightly. Try experimenting stopping the striking sequence at various stages, ie earlier than you would normally, you might find that the little bit of kiln striking will bring the TN to your preferred colour.  ;)
Title: Re: At my wits end - overstriking
Post by: helbels on March 20, 2011, 02:16:06 PM
Thanks Bev, that makes complete sense - I will try again and am feeling a bit more hopeful now!