Frit-Happens !

Lampwork => Common Problems => Topic started by: Shirl on March 09, 2011, 11:47:54 PM

Title: Cracked beads
Post by: Shirl on March 09, 2011, 11:47:54 PM
I usually batch anneal, but for the first time this morning I put my kiln on and garaged and then annealed as I wanted to make some hand shaped lentils and they cracked if cooled in the vermiculite when I have made them on previous sessions.

NOT a good result today, just got them from the kiln and found most of the lentil shapes cracked :'( :'(   The round beads I made at the same time were all fine.

I am not sure why this happenned. Did I get them too cool while shaping?

(http://i1129.photobucket.com/albums/m517/scottam/broken226.jpg)

Title: Re: Cracked beads
Post by: Veebee on March 10, 2011, 12:05:57 AM
Aw, gutting. Yup, that's a thermal crack, and it means you let them cool too much when shaping. After pressing/shaping etc, give the bead a good heat bath to a dull glow to help avoid this, but not so hot that the glass goes gloopy and loses shape. Have another go, they're looking good!
Title: Re: Cracked beads
Post by: sarah t on March 10, 2011, 12:30:11 AM
cracks like that are usually thermal so ''got to cool when shapping''  or adding layers a good shout i reckon ....

the remedy is a bit tricker as i am not sure when its cooling to much ......

dont press/squish for too long ...i use the press bottom to shape and only do a final press using the top (if it has one) once if possible !...re heat in between each shapping or adding more glass but not to much or you lose the shape ...after the final press and its ready for the kiln i heat it up again in the top of the flame and give it a final bit of heat ......make sure you remember the top and bottom of the bead as well as the back and front ...i kind of rock the bead to and fro but that could just be me !

the other reason is could be they are too thin...a little less squishing could help

its also sometimes tricky to get the core back to a compatable heat when encasing ...so maybe try doing the shaping without encasing till you have had a bit more success ...

i am afraid its practise practise practise ........ but it will suddenly click ...and garaging is usually a bit more forgiving than other forms of cooling with bigger beads...shame they were looking good

good luck  

Title: Re: Cracked beads
Post by: Shirl on March 10, 2011, 04:35:02 PM
Thanks so much for the advice :) :)

I have had another go today, but was a bit paranoid about letting them get too cool, so much so that one of my beads must have been a bit too hot and it stuck to another one as I put it in the kiln :o

Another lesson learnt
Title: Re: Cracked beads
Post by: turnedlight on March 10, 2011, 04:51:35 PM
You don't have to wait for the glow to go completely before putting them in the kiln - just hold it so it is off the floor for a few moments til the glow goes and then you can put it down. I do this especially with the bigger beads.
Title: Re: Cracked beads
Post by: Shirl on March 10, 2011, 06:02:22 PM
Quote from: turnedlight on March 10, 2011, 04:51:35 PM
You don't have to wait for the glow to go completely before putting them in the kiln - just hold it so it is off the floor for a few moments til the glow goes and then you can put it down. I do this especially with the bigger beads.

I never thought of this...thanks :)
Title: Re: Cracked beads
Post by: ♥♥Tan♥♥ on March 10, 2011, 07:39:33 PM
what a shame, there are some lovely beads there :'(
Title: Re: Cracked beads
Post by: Margram on March 10, 2011, 10:20:33 PM
If you clean them really well you can slump them into lovely cabs...
Title: Re: Cracked beads
Post by: TheJanie on March 10, 2011, 10:40:01 PM
Quote from: Margram on March 10, 2011, 10:20:33 PM
If you clean them really well you can slump them into lovely cabs...

That's what I've been mostly doing this week :)
Title: Re: Cracked beads
Post by: Lush! on March 10, 2011, 11:03:52 PM
Oh what a shame  :(

What size are your mandrels? They look quite thick, which would mean that the glass either side is thinner. It may help to use a finer mandrel - I use 1.6mm with my lentil press.
Title: Re: Cracked beads
Post by: Shirl on March 11, 2011, 10:30:47 AM
Quote from: Lush! on March 10, 2011, 11:03:52 PM
Oh what a shame  :(

What size are your mandrels? They look quite thick, which would mean that the glass either side is thinner. It may help to use a finer mandrel - I use 1.6mm with my lentil press.

These were made on my new 1.6 mandrels :o
Title: Re: Cracked beads
Post by: Shirl on March 11, 2011, 10:38:32 AM
Well ......I just got my beads from the kiln this morning and I only tried one lentil ( the same glass and style as the last cracked ones for comparison) and some other round beads.......YEY no cracks, so I spent a bit of time looking at my creations and then them put them into water to remove the mandrels...... I let them soak a few mins and when looking at my lentil .....OH NO.. it is Cracked :'(  in exaxctly the same way as the last ones!

I put it in the kiln while it was quite hot, and took great care to make sure it was heated through before putting it in.

I thought I had done everything right this time....but no joy.

At least I only got one cracked! (but I only made one lentil)

If I carry on like this I will have so many half beads i will have to make them into cabs (scary) or stick them round a picture frame!
Title: Re: Cracked beads
Post by: TheJanie on March 11, 2011, 12:34:47 PM
Quote from: Shirl on March 11, 2011, 10:38:32 AM
If I carry on like this I will have so many half beads i will have to make them into cabs (scary) or stick them round a picture frame!

I thought slumping them into cabs was scary - then finally got the courage to start experimenting this week.  I'm still trying to get the program right, but I'm getting there!

Before that, I stuck magnets on the back of half-beads and decorated my fridge with them :)
Title: Re: Cracked beads
Post by: sarah t on March 11, 2011, 01:22:55 PM
bugger  >:(
dont know what to suggest now ....maybe different glass ??..could be a compatabilty /heat issue  ?...you could try making a few in just one type of glass

or maybe kiln ???...what temperature /schedule are you using ?

Title: Re: Cracked beads
Post by: turnedlight on March 11, 2011, 04:01:34 PM
What glass are you using?
Title: Re: Cracked beads
Post by: Shirl on March 11, 2011, 04:19:52 PM
I used CIM blackcurrant base, wrapped in silver leaf, swiped with Triton and encased in Eff 006 clear. Then squished with my mashers as I dont have a press. (yet)

My schedule in my Paragon SC3 with bead door was



Segment 1: Ramp1 990 deg C Temp1 510 deg C Hold1 12 HRS

Segment 2: Ramp2 FULL Temp2 520 deg C ** Hold2 1 HR

Segment 3: Ramp3 50 deg C Temp3 370 deg C Hold3 0000mins

Segment 4: Ramp4 0000

Title: Re: Cracked beads
Post by: turnedlight on March 11, 2011, 05:07:11 PM
 I dunno.. maybe it could be too much silver in your beads, in the reduction of the Triton, added to the silver foil? In the past I've had the occasional cracks with a really metallic shiny encased Triton bead, (I encase in 006 like you) and wondered if there's such a thing as too much silver!
I garage my beads, I go straight to 520, hold it there whilst adding beads in, then at the end I leave it for 30 mins to an hour depending on the beads and ramp down. I've not tried garaging at 510, it doesn't sound too low but maybe you could try going straight to 520.
Title: Re: Cracked beads
Post by: Veebee on March 11, 2011, 05:16:09 PM
I hold for a while after bringing down through the stress ranges, I would suggest your hold 3 should be for maybe 20 mins just to let them settle. Also, were they cool when you got them out of the kiln? (sorry if that seems to be a condescending question, it's not meant to be!) The centre of the bead holds the heat, if the bead was still warm on the outside when it went into the water then it will probably still have been warmer than you think on the inside... just another thought.
Title: Re: Cracked beads
Post by: turnedlight on March 11, 2011, 05:19:34 PM
Ooh yes, I missed that, it's not stopping at 370 and letting the stresses even out.
Title: Re: Cracked beads
Post by: Shirl on March 11, 2011, 05:53:24 PM
This was the schedule for the first batch from fritpedia

Good for COE 90 and 104 glass

Segment 1: Ramp1 900 deg C Temp1 500 deg C Hold1 12 HRS

Segment 2: Ramp2 FULL Temp2 520 deg C ** Hold2 1 HR

Segment 3: Ramp3 78 deg C Temp3 370 deg C Hold3 0000mins

Segment 4: Ramp4 0000


For the second batch I changed ramp 3 to 50 deg  instead of 78 as I thought the slower cooling might be better.

I did not know you had to hold  at 370 deg. I thought it just cooled down naturally from there. The beads were left overnight so should have been well cooled
Title: Re: Cracked beads
Post by: Veebee on March 11, 2011, 05:58:52 PM
I would definitely hold for a short while at 3, then you can just let the natural cooling happen.
Title: Re: Cracked beads
Post by: Shirl on March 11, 2011, 06:01:09 PM
Quote from: Veebee on March 11, 2011, 05:58:52 PM
I would definitely hold for a short while at 3, then you can just let the natural cooling happen.

Thanks Veebee, it wont hurt to try that, and fingers crossed it might work :)
Title: Re: Cracked beads
Post by: sarah t on March 11, 2011, 06:02:54 PM
we will get you there in the end  ;)
Title: Re: Cracked beads
Post by: Shirl on March 11, 2011, 06:05:56 PM
Oh I hope so  ;D

I think I might try doing some simple test beads in different colours to see how they work out
Title: Re: Cracked beads
Post by: Veebee on March 11, 2011, 06:07:21 PM
Lentils, of course..........
;D
Title: Re: Cracked beads
Post by: Pat from Canvey on March 15, 2011, 11:52:30 AM
I'm not sure why you have the Segment 1 at all. I go straight to 520C ramping at FULL. After the last bead goes in, I hold for an hour, skip the program and then ramp down. Down takes 3 hours or so after the skip. No problems with any sort of bead including very large ones. I programmed mine from the manual that came with the SC2 kiln. Take beads out at about 65C hold for a few minutes to admire and then dunk in water.
Title: Re: Cracked beads
Post by: Shirl on March 15, 2011, 03:12:16 PM
Quote from: Pat from Canvey on March 15, 2011, 11:52:30 AM
I'm not sure why you have the Segment 1 at all. I go straight to 520C ramping at FULL. After the last bead goes in, I hold for an hour, skip the program and then ramp down. Down takes 3 hours or so after the skip. No problems with any sort of bead including very large ones. I programmed mine from the manual that came with the SC2 kiln. Take beads out at about 65C hold for a few minutes to admire and then dunk in water.

Thanks Pat. :)
If I ramp at full my kiln overshoots and ends up at about 550, so I just heat up a bit slower.

I expect there are lots of ways to do it, all being a different variation.