Frit-Happens !

Lampwork => Common Problems => Topic started by: Kay24 on February 21, 2011, 09:23:03 PM

Title: Bead Release Problems
Post by: Kay24 on February 21, 2011, 09:23:03 PM
Hi All

Just after a bit of advice please, I use fusion bead release and tend to dip as I go along, I spent all day yesterday making beads and about 6 mandrels coated in it cracked, some nearly as soon as I started making a bead others half way through and some just at the blooming end, I got so frustrated, what am I doing wrong????? 

I dip them and flame dry but quite alot of the times they crack, I wash my mandrels after I take the previous beads off them in a bit of fairy liquid (should I not be doing this?) is there anything else I need to be doing?? I don't always use them straight away once they are washed but I don't dip them until I am going to use them, I found if I leave them dipped for too long they all tend to break.

Also my bead release has gone very thick, I am about just over half way down the tub, could the thickness be causing the problem?  I did add a tiny amount of water to it last week but was scared about watering it down too much.

Help pls

Thanks K
Title: Re: Bead Release Problems
Post by: ♥♥Tan♥♥ on February 21, 2011, 09:27:26 PM
If I flame dry I get this problem if I dry too quickly, so I start at the metal end and let the heat kind of push its way up the bead release slowly.

The other thing is it sounds as if your release is a bit thick, I boil a kettle, let it cool to warm then thin the release and bung a couple of fuglies in the pot, don't worry if you thin too much just leave the top off overnight
Title: Re: Bead Release Problems
Post by: Kay24 on February 21, 2011, 09:29:37 PM
Thanks Tan will give this a try, off to boil the kettle now  :D
Title: Re: Bead Release Problems
Post by: MangoBeads on February 21, 2011, 09:54:34 PM
Totally agree with Tan i don't get on with flame drying at all and it sounds too thick so a mixture of the two is causing your problems for sure. I use Fusion plus and have the same problems so don't flame dry and make sure it's not too thick. BUT i swear by it its good stuff one s you get to know it ::)
Title: Re: Bead Release Problems
Post by: Les on February 21, 2011, 09:57:53 PM
I find that if I flame dry immediately after dipping, I get cracks and bits of release pinging off .... if I leave the mandrels for around 30 to 45 minutes after dipping, they flame dry just fine :)

If your release is too thick though, it will need thinning or else it will crack, no matter what you try.
Title: Re: Bead Release Problems
Post by: helbels on February 21, 2011, 10:01:10 PM
I flame dry all the time with no problems, but I heat the release by just wafting the mandrel in and out of the flame, rather than just heating it in one spot directly.
Title: Re: Bead Release Problems
Post by: rocky on February 21, 2011, 10:13:01 PM
I usually dip a whole load of mandrels after I've finished at the torch, so they slow-dry for the next session. The bead release doesnt seem to crack that way.
Title: Re: Bead Release Problems
Post by: Kay24 on February 21, 2011, 10:16:30 PM
Thanks all I watered it down a moment ago just hope I didn't do it too much, I will try any make sure I dip them and hour before I start, will try it out tomorrow :)
Title: Re: Bead Release Problems
Post by: ♥♥Tan♥♥ on February 21, 2011, 10:21:49 PM
Shake it well then dip one mandrel, give it a minute then have a look, if the release looks crazed then its too thin and needs to sit around with the lid off for a while. If you are impatient to get going you can shortcut around it by double dipping.
Title: Re: Bead Release Problems
Post by: Ness on February 22, 2011, 12:01:10 AM
I wouldn't worry too much about having coated rods hanging around either - I've used rods that were dipped and air dried weeks before and haven't had any problems with cracking. 

When I do have to flame dry I take it easy and do the wafty thing, too ;)

Also, do you make sure you heat all of the bead release that you are going to cover with glass?
Title: Re: Bead Release Problems
Post by: DeanWilson on February 22, 2011, 12:08:18 AM
That's really weird with fusion- for me anyway! My old bead release was given to me and completely un-flame-dryable :P So now that it's an option I love it! Lampworking on the go; without the 3 hour preparation time :P

I put the lid on (VERY important!!) and just give the tub a really good shake. I dip them all, sometimes doing them twice (not drying in between, just in once, out, twice :)- thanks Gemma!), especially my 2 5mm ones for my BHBs!

I get to my desk and ALWAYS flame dry them! And I do it as I need them- I do do it slowly but not that slowly now that I think about it! :S Mine is always very well mixed before I use it maybe that could be a cause?

Dean ;D x
Title: Re: Bead Release Problems
Post by: sarah t on February 22, 2011, 12:30:50 AM
i have never had much luck with flame drying .....i dip the night before ......and i bring any left in from the shed (along with the oxycon) at the end of a session.... they dont like cold or damp ....i do that shelf stacker thing of using the older ones first so they are never more than a couple of days old

i use a green scrbby thing and water to clean my mandrels dont know if it makes much difference but in my mind gives a bit of a surface for the realease to grab on to

Title: Re: Bead Release Problems
Post by: ★★Terri★★ on February 22, 2011, 07:55:10 AM
I use my own bead release and use both methods of drying - for flame drying I gently waft the mandrel in and out of the top of the flame.  Initially it starts to steam a bit, as this stops I waft again and stay longer in the flame as the release gets dry.  It pings off only if I get too hot to quickly or if there is a thicker bit, say from a drip/run.
Title: Re: Bead Release Problems
Post by: Lotti on February 22, 2011, 08:29:50 AM
Use the fusion plus that Manda mentioned (and I got from her) and it is WONDERFUL as long as I treat it right (not too thick etc).  I can't torch every day cos need to get some work done sadly, but after each session I clean the mandrels and redip them ready for next time whcih in this case will be two weeks :(.
Title: Re: Bead Release Problems
Post by: Pat from Canvey on February 22, 2011, 09:05:32 AM
For the last few months, I've started to remove the dried bead release from the mandrel after the bead is made by rubbing it through my fingers straight into the bin. I find that the beads then come off the mandrel after say only a 10 min soak in water. I clean any other release off the mandrel in water only but always dry each mandrel on paper towel.
Title: Re: Bead Release Problems
Post by: Sarah on February 22, 2011, 05:39:48 PM
I use fusion and have no problems with flame drying. But I usually let the mandrels stand for about 10 - 20 minutes before I use them and I dry them behind the flame so that they dry slowly.

If you water your release down too much just leave the lid off for a while and it will thicken again.

Sarah
xxx
Title: Re: Bead Release Problems
Post by: ★★Terri★★ on February 22, 2011, 09:48:29 PM
Quote from: Pat from Canvey on February 22, 2011, 09:05:32 AM
For the last few months, I've started to remove the dried bead release from the mandrel after the bead is made by rubbing it through my fingers straight into the bin. I find that the beads then come off the mandrel after say only a 10 min soak in water. I clean any other release off the mandrel in water only but always dry each mandrel on paper towel.

Please be careful with dry bead release it has a lot of silica in it - which breaks up into very fine airbourne particles and will cause serious damage to your lungs when inhaled.  You should always take care if you are brushing it off when it's dry and wear a dust mask/ventilator and use ventilation, or keep it damp to prevent dust.  The dust from breaking it up when dry will stay floating in the air for hours.