I have had a love/hate relationship with silver glass for years...... i love it it hates me  ;)

decided to give the fire opals a go, it went well, great colours, batched annealled them on my usual schedual 520 c, came out crappy  ::)
looked at the double helix striking guide and they advise 940f (504 c), what temp do you use?
sandy
Title: Re: annealling temp for ekho
Post by: julieHB on February 06, 2011, 10:07:50 AM
I garage at 500deg C, and anneal at 510 deg C, and have never had a problem. I think my kiln fires a bit cold, though, so my feeling is that the actual temperature is lower than that.

you could try to anneal at 510 or 500, and see if you find the temp. that does not take away reduction shine or strike the glass. I know some lampworkers anneal the silver glasses as low as 480 deg C.

you might find this useful: http://envisionsf.blogspot.com/2009/04/silver-glass-101-annealing-temperature.html

HTH  :)
Title: Re: annealling temp for ekho
Post by: Fruddy on February 06, 2011, 11:35:00 AM
I used to garage at 510 and then anneal at 520 for an hour, but I took Julie's advice above - especially as my kiln does have a tendancy to overshoot by about 10 degrees.

I used to find that glasses like Luna 2, Ekho, Terranova etc. used to go in brightly coloured and come out a murky brown or cream.

I now garage at 490 and then put the temp up to 500 to anneal for an hour.
Title: Re: annealling temp for ekho
Post by: flowerjasper on February 06, 2011, 12:38:13 PM
thanks will drop the temp and give it another go  ;)
sandy x
Title: Re: annealling temp for ekho
Post by: Ness on February 07, 2011, 10:59:11 PM
After a slip of the finger trying to advance my program I garage at 517, but anneal at 520.  I've never have any problems with changes to my silver glass.  I may have  a go at lowering my temp too, just as a test. 