I am trying to encase some Double Helix in clear glass as per some tutorials I have seen. I have no real trouble in getting the colours to show up and when I encase the bead in clear glass all seems well ( the clear is nice and clear, not scummy ) but they crack ( along the line of the mandrel ) when I leave them. I have left them in a hot slow cooker with vercimulite and well as garaging them in a kiln, showing 300 deg C as the temperature, I then ramp the temp upto about 550 ( at 200 deg per hour ) hold for hour and a half then allow the kiln to cool over the next two or three hours or more. My sucess rate is about 20% not cracked. any ideas please ?
Gordon
Which clear are you using?
Depends which clear you are using - I will only use effetre 006 as I have had problems (as have others) in the past with Lauscha and CIM. Reichenbach clear is OK too or even DH own clear (which is horrendously expensive!!!)
Kazx
Not sure what clear it is I bought it at a bead fair from Martin. I do know it goes scummy if it gets slightly too hot, something I'm prone to do as I'm still a beginner, I only manage to get a 3 or 4 hours per week torch time.
Are you sure it's not borosilicate? Is it labelled at all?
It's not labelled, and I'm sure it's not borosillicate as I am using a minor with one Oxycon and I have no problems melting it.
If it's cracking along the mandrel it sounds like a thermal crack - ie it's got too cold before you have put it in the vermiculite.
But it could also depend on the size of bead and if it's pressed.
If you press a bead, the press suck sout a lot of the heat so you need to warm it up, again after pressing (not glupy hot so it melts) as the outer part of the bead will have cooled a lot faster than the inner temperature.
As the others have said, as a rule silver rich glass doesn't generally get on well with lauscha clear. I use the std 006 Effetre and it works just fine for me!
Another thought - don't know if this makes a difference, but I normally garage at a higher kiln temperature - 500 degrees
Ditto make sure its 006 :)
300 degrees C is far too low for your garaging, and 550 is a bit too high. It should be more like 490-500 and 520 (though I both garage and anneal at 510). Do they have a slight glow when you put them into the kiln?
Quote from: Kalorlo on January 17, 2011, 03:43:59 PM
300 degrees C is far too low for your garaging, and 550 is a bit too high. It should be more like 490-500 and 520 (though I both garage and anneal at 510). Do they have a slight glow when you put them into the kiln?
Yep - I meant to say that too!
Ok off to Martrins for some "006" and I'll garage at a higher ,490 .. 510 deg C, and see how I go Thanks a million :0)
G
I garage at 520 and the only cracks I ever get are those annoying incompatability cracks from time to time, if I have picked up some rogue bullseye
Quote from: Gordon on January 17, 2011, 05:16:03 PM
Ok off to Martrins for some "006" and I'll garage at a higher ,490 .. 510 deg C, and see how I go Thanks a million :0)
G
These measures should do the trick.
The 006 crystal Clear came today, I've had another go this evening and no cracking, thanks a mill... :) :)
G
I was working on the encasing skills(lol) yesterday and noticed that I was getting some 'thermal cracking' with silver glass. This is the first time I've got silver glass to do something for me - yay - and then it cracks. Getting to the point - I think I was letting the glass on the mandrel get too cold while melting the clear and as soon as I put the hot encasing glass on I felt and heard the bead crack on the mandrel. :'( I suppose it's just part of the process of learning how near to keep the bead to keep it hot enough without getting in back in the flame and losing the reduction.
I'm having a little trouble keeping the reduction on "Electra" I think I'm letting it get too hot when I encase it but it's early days I'm sure we'll 'crack' ;) it soon enough
G