Lampwork => Common Problems => Topic started by: Sarah A on January 09, 2011, 09:40:12 PM

Title: Is my hothead hot enough???
Post by: Sarah A on January 09, 2011, 09:40:12 PM
Hi after looking at some video's of hotheads I have found my flame does not glow yellow when I put glass into it.  It also seems to take ages to melt the glass and when I try and wrap it round a mandrel it is very stiff and not runny like I thought it would be.  If anyone can give any suggestions, they would be much appreciated.  I am using propane and not map gas that was used in the vidoes, not sure if this makes a difference.
Title: Re: Is my hothead hot enough???
Post by: SilverGems89 on January 09, 2011, 09:44:32 PM
do you have the tap on the torch itself fully open? i had problems with mine before when i didnt have it open fully, so now its all the way open and i control the flame with the regulator
Title: Re: Is my hothead hot enough???
Post by: jammie on January 09, 2011, 10:53:26 PM
Mine has been losing pressure,  I think its with the cold, some days its better than others. I have torch full up and regulator full up and its always less hot at the end of the tank or nearly at the tank.
Title: Re: Is my hothead hot enough???
Post by: Blue Box Studio on January 10, 2011, 12:11:54 AM
Sounds like the problems I had when I started.  I don't have my torch fully on but I do turn the gas fully on but the regulator is turned all the way down and back up about 1 full turn, if that makes any sense.  When the gas tank gets low and it's cold I find it is less effective but am assuming you are OK for gas?  I'd try turning the regulator up and down until you get the right pressure.  Let us know how you get on.
Title: Re: Is my hothead hot enough???
Post by: paintboxcrafts on January 10, 2011, 09:33:14 AM
The lack of glow when you put the glass in the flame may be as simple as the fact you are wearing your diddy's and the cameras
doing the filming are not.
Title: Re: Is my hothead hot enough???
Post by: Kalorlo on January 10, 2011, 12:16:13 PM
If you peer at your flame over your diddys for a sec when you put the glass in it, you should be able to see the orange flare. If there isn't one, try moving about in the flame a bit until there is.

You could also try using Effetre white. It's one of the runniest glasses and should give you a feel for where the softer end is. Transparents are stiffer. You might just need to slow down a bit and give them more heat before you try to wind them on.

Silly question, but are you using coe 104 glass? 96 and bullseye (90) and so on are stiffer. Still usable, though.
Title: Re: Is my hothead hot enough???
Post by: Sarah A on January 10, 2011, 06:30:33 PM
Hi thanks for the replies.  I am using effetre.  I will look over the glasses and see if I can see the yellow glow.  My gas bottle is new apart from the 3 hours I have used it to make 4 beads.  I have turned the torch open as far as it would go and turned the gas bottle on fully.  Have had a bit of a fiddle with the regulator but will have another go tonight and have another fiddle.  I will also try using the white and see if that melts any quicker.  Will let you know how I get on and thanks again for all your advice.
Title: Re: Is my hothead hot enough???
Post by: SilverGems89 on January 10, 2011, 06:40:40 PM
Also remember screw the regulator DOWN to open it, i always forget that bit  ;)
Title: Re: Is my hothead hot enough???
Post by: dangerousbead on January 10, 2011, 07:07:34 PM
Just a thought, is your torch a real Hot Head? I'm only asking what seems a daft question cos when I changed to bulk I had the same problem and the reason was because my torch was actually a so called HH from Fireworks. Fine on small tanks rubbish on bulk.
Title: Re: Is my hothead hot enough???
Post by: Sarah A on January 10, 2011, 09:17:51 PM
Have just made a bead in white, followed all the advice re turning hh and gas on full regulator down and then one turn up and the flame seemed much bluer without the ble ring near the torch which there had been.  Glass melted very quickly and seemed much runnier.  Think I'll stick to doing this in future.  Hopefully my hh is a proper one got it from tuffnells.

Thanks again to everyone for their advice on this.  Now can't wait to make more beads another night!!