I bought a couple of 5mm mandrels from Tuffnells and tried using them tonight. I used fusion bead release as usual but the release on both mandrels cracked. One of them had been single dipped and the other was double dipped.
I was reluctant to continue in case I could not get the beads off but it would be helpful to know if this is a common problem and whether there is anything I can do about it.
Thanks
Sandra
Did you give the new mandrels a bit of a scour? New mandrels often are not completely clean of oil etc so always a good idea to scour them before use :)
Did you rough up your mandrels first (using a scourer or something similar). Someone else suggested in this cold weather to let them dry inside.
Hope that helps!
I have this issue too, I have used mine a few times now and use Fosterfire Heavy Duty, and mine crack every time.
I always manage, slowly, to finish the bead, but don't dare tip it in case it falls off.
I find my fusion cracks sometimes if I marver heavily, or use my charm box press (which I use more like a bead roller, think the brass is too grippy)
a normal gently shaped bhb won't usually crack the bead release for me.
how diluted is your bead release? this can have an effect too.
I single dip, but thickly, ie, undiluted, and air dry (and I'm indoors)
The thing to do is get a jar of water by your torch and heat the new mandrels until they go black, and quench them in the water. Do it twice, and it improves the sticking power of the release. I use fusion, and if I do this it is usually fine. I now also double dip in fairly thin release.
Thanks for the advice. It is a while since I bought any new mandrels and I had completely forgotten about scouring!!
Will try the heating and cold water too.
Thanks again
Sandra
I'm using fusion and haven't had any problems - only got the one BHB mandrel though, so I can only make one at a time! Mine are also usually doughnuts - no BHB press or roller yet.
I had this problem with some mandrels the engineering dept at work cut me, turns out they were coated with a thin layer of oil, so a quick wash in soapy water and a rub with a pan scourer and they were fine.
kath