Frit-Happens !

Lampwork => Common Problems => Topic started by: ScarletLeonard on November 10, 2010, 09:41:37 PM

Title: So the Twisty thing
Post by: ScarletLeonard on November 10, 2010, 09:41:37 PM
I have to have read a number of tutorials, I've been shown how to make them and been swatting up on youtube.

Methods I've tried
toothpasting base rod with second colour (in one place, two places, 4 places.)
making a two tone barrel (both ways round)
banding two rods together and melting.
twisting the second colour round the base rod then attempting to pull like a normal stringer (last resort)

I've tried all of these using tweezers a boro punty and a 104 punty and I still can't seem to get more than 2inches of a twisty. If I do get one longer the twist is different, it ends up to thin or just plain goes wobbly.

A huge gather of glass seems to work well because I can keep ducking that in and out of the flame and it doesn't get too hot but I lose momentum
a small gather like I would use for a normal stringer just doesn't stay in the right stage of meltyness for me.

Can't help but think there is something i am doing wrong.

HELP
Title: Re: So the Twisty thing
Post by: Redkite on November 10, 2010, 10:47:01 PM
A method I learned at the weekend (thanks to Lush Julie)

Take 3 rods and put an elastic band around them to keep them together.

Optional: use clear to encase the last inch of the combined bunch of rods.

Take a 104 clear rod, heat the end and press it onto a marver to make the end as wide as the bunch of rods.

Heat the end of the bunched rods and the punty and attach the two together, so you have the bunch of rods in one hand and the clear rod in the other.

Heat the (encased) end of the bunch of rods until they are glowing evenly and starting to get a bit saggy.

Take the glass out of the flame, wait for a couple of seconds, then start twisting with both hands.

Gradually pull the two ends apart, while still twisting.

The mistake I made was to pull too hard and too quickly. Concentrate on twisting first, then pull.

HTH
Title: Re: So the Twisty thing
Post by: mizgeorge on November 10, 2010, 11:30:06 PM
This technique works brilliantly IMO - both encased and not. I was hugely impressed :)
Title: Re: So the Twisty thing
Post by: Redhotsal on November 11, 2010, 12:04:36 AM
Here's a dead easy way to pull twisty:

Take two grotty and bent old mandrels (they can be brand new ones, but since you won't be able to use them for bead making in the future you may as well use old ones.)

Take a colour that you want for the twistie and heat up the tip of the mandrel. Wind hot glass onto the very end of the mandrel like you were making a bead. So, it's like a bead on the very end of the mandrel. Don't use any bead release, go straight onto the bare metal and try and make a nice round ball at the very end of the mandrel. Try to keep the ball on the very end of the metal, you want lots of glass on it's own in a ball at the end of the mandrel - the more you spread it down the mandrel the less length of twistie you'll get.

When you've got a "ball on a stick" (and make sure the mandrel has only poked its way into the ball by about 2mm at the most) take another contrasting colour and apply a nice thick stripe running all the way around the ball. Start at the point where the glass meets the mandrel and run the stripe all the way around until it meets the mandrel on the other side of the ball. You can do this with stringer but it needs to be thick so you may as well use the rod.

Melt this in gently so its fully melted into the ball. It's a challenge to do this and keep the ball on the end of the stick, but really that's the hardest bit of the whole process. Keep taking the ball out of the flame to give the stripe a chance to melt in.

When you have done this, let the ball cool a little so it goes solid and take another grotty mandrel. Heat the tip until it glows and also heat the "open" end of the ball until it glows and then push the new mandrel into the ball by about 2mm. The new mandrel should be in line with the original mandrel so that they will now form the two handles. Holding the ball by these two handles you can now heat it until it is glowing orange.

Take it out of the heat before it goes too floppy, let it rest for about three or four seconds, start to pull the handles apart first and then twist, twist, twist.

Because you haven't got the glass rods to worry about melting it's a lot easier to do and also as the mandrels are a lot thinner than glass rods it's easier to twist 'em. I get twice the length of twistie using this method than I do using glass rods alone and for some reason it seems a lot more leisurely. I also make silvered ivory stringer and quite a few Murrine this way.

Give it a go - it's dead easy and lots of fun. And to get the end pieces of glass off the mandrels afterwards just heat then up and dunk into water.
Title: Re: So the Twisty thing
Post by: pixiewillow on November 11, 2010, 08:01:38 AM
Not sure if these photos will help any put I demonstrated twisties while I was in Holland last month....

Basically everything that Sal said but on a big hole mandrel  ;D

Okay this was making a murinni but I build my twisties exactly the same way on the end of a big hole mandrel
(http://farm5.static.flickr.com/4033/5165738869_6dce14756b.jpg) (http://www.flickr.com/photos/23010246@N08/5165738869/)
P1120609 (http://www.flickr.com/photos/23010246@N08/5165738869/) by pixiewillowdesigns (http://www.flickr.com/people/23010246@N08/), on Flickr

I think you can just make this out... using a 8-10mm rod make a punty and attach
(http://farm5.static.flickr.com/4020/5165739023_a76404d1e9.jpg) (http://www.flickr.com/photos/23010246@N08/5165739023/)
P1120614 (http://www.flickr.com/photos/23010246@N08/5165739023/) by pixiewillowdesigns (http://www.flickr.com/people/23010246@N08/), on Flickr

When you pull and twist make sure that the mandrel is higher than the punty si the heat travels up into your gather and helps to keep it moving a bit longer. If the punty was higher you run the risk of melting the rod and just pulling a stringer lol!

(http://farm5.static.flickr.com/4154/5166340606_234e6df2b9.jpg) (http://www.flickr.com/photos/23010246@N08/5166340606/)
P1120624 (http://www.flickr.com/photos/23010246@N08/5166340606/) by pixiewillowdesigns (http://www.flickr.com/people/23010246@N08/), on Flickr
Title: Re: So the Twisty thing
Post by: Tills on November 11, 2010, 08:02:25 AM
DITTO to Julie's (lush) way, I can now do lovely twisties  ;D
Title: Re: So the Twisty thing
Post by: ScarletLeonard on November 11, 2010, 10:09:41 AM
Looks like I have a lot to try again tonight

Sal I haven't tried 2 mandrels yet and it does sound easier.

I'll try multiple rods again too.

Though the mention of allowing the heat to rise when I pull stringers I do hold it nearly vertical but with my twisties I have been horizontal (concentrating to much on the twisting) that could be why I seem to be getting less pull from my gather.

I will get this right!

Thanks again everyone.
Title: Re: So the Twisty thing
Post by: ♥♥Tan♥♥ on November 11, 2010, 10:17:33 AM
Lorna you look dead impressive ;)
Title: Re: So the Twisty thing
Post by: Kalorlo on November 11, 2010, 10:24:05 AM
Yes, this. I use the fat end of stainless steel chopsticks instead of old mandrels but it's the same idea. I've done the rubber banding method once (with 4 commercial stringers and a chopstick) and that worked pretty well too. I didn't have much luck with using glass rods as punties - they always get too cold and fall off on me, or I worry about melting them. My problem with my first tries was not getting my gather hot enough. Make a nice big one and heat it all up!  ;D

The benefit of the chopsticks is that the curved ends mean that when the twistie cools, the ends just fall off the metal.
Title: Re: So the Twisty thing
Post by: beadysam on November 11, 2010, 02:32:06 PM
I've got some chopsticks I bought with a view to selling them for twisty making.  However, they are thin hollow crappy ones so there is no way I can sell them.  If anyone orders from me fee free to add a note asking for a pair of chopsticks and I'll pop them in.  They are very thin metal though so don't go mad with the heating or you will burn through them.