I have been making spine beads and had a problem with the first two, I think as I used a frit base and overdid the amount. They both split directly across, horizontal to the mandrel and I hadn't annealed them. This time I made two with silver glass, one with triton and the other Kalypso, garaged them on the usual schedule in my SC2, all fine. I reamed them last night, and put them on top of the piano where all my new beads live.
Five minutes ago, I was sitting at the pc, minding my own business when the triton bead, um, broke in half with a bang, sending one half flying across the room. I've never seen the like ??? And I definitely didn't roll it in dynamite or anything like that, before anybody asks ::)
So what have I done wrong?
Hiya,
Were the beads encased and if so, what clear dis you use?
Some clears don't play nicely with silver glass.
Helen
Hmmmm - it could be the clear on the silver glass, but it also sounds like a thermal crack - ie they've gotton cold to quickly!
They were encased and I used CIM on both - and it was the annealing schedule given in the SC2 manual which I used - I've never had a problem before with beads breaking a day later, but I've never annealed silver glass before. This is the first time I've ever got it to play nice, so I'm a bit sad to lose it.
It doesn't sound like an annealing problem if your other beads are fine (but just for info - you can find a schedule here http://www.frit-happens.co.uk/wiki/Annealing)
As far as I'm aware, CIM glass should be fine - my guess was that they cooled too much before going into your kiln or fibre blanket! Although another point to consider, if they were pressed beads, were they pressed too thin perhaps??
Do you have any pictures?
I shall have a go at piccys, and load them up later, thanks
Maybe after pressing you didnt get them hot enough again or looked at them for too long (I have done this) before garaging.
One of mine (spine bead attempt 2 ) cracked after annealing, I thought it was because it took so long to add the clear before pressing but I didnt notice it till it came out of the kiln. It was a vertical crack.
Righty ho, this is the broken bead, excuse my photography
(http://farm5.static.flickr.com/4144/5117315205_e33a219fc8.jpg) (http://www.flickr.com/photos/54880518@N08/5117315205/)
SDC10241 (http://www.flickr.com/photos/54880518@N08/5117315205/) by awrylemming (http://www.flickr.com/people/54880518@N08/), on Flickr
and this is the survivor
(http://farm2.static.flickr.com/1395/5117312523_55a9e7c49b.jpg) (http://www.flickr.com/photos/54880518@N08/5117312523/)
SDC10258 (http://www.flickr.com/photos/54880518@N08/5117312523/) by awrylemming (http://www.flickr.com/people/54880518@N08/), on Flickr
and I was really good with these two Kay, as I made that mistake with the first two, straight in the kiln ::)
It might, however, be the amount of time it took to get on the clear, but I can't see a way round that with a hothead. And I used the same technique with the surviving bead. It's more the landing on the other side of the room that surprised me. ???
And I wish I could find a way to make the pictures smaller! Aaaargh, I hate computers.
The bead pics are a perfect size, as for the other side of the room it just 'pinged'
I am baffled, did you reheat to a glow after you pressed it, how wide is it, is the bead at least double the width of the mandrel?
Shame :( The crack runs from hole to hole, along the mandrel line? I get this when I don't keep my tree beads warm enough (usually when I forget to warm the back of the bead because I've been distracted by decorating the front). Once you've encase the bead, I think you need to get it back up to glowing, then allow to cool again at the end of the flame before putting in the kiln.
That cracked one looks the same as mine and i,m pretty sure it was not keeping it hot enough as i was melting a thick rod of clear on a hot head and it took yonks.i thought I would encase in smaller goes rather than winding on in a thick coil.
The bottom ones pretty never had the pinging....ghosties maybe ::)
That looks like a 'i got too cool' crack to me - what bad luck ???
Quote from: MangoBeads on October 26, 2010, 05:08:30 PM
That looks like a 'i got too cool' crack to me - what bad luck ???
I think so too - so you need to give it some more heat after you press it! At least you know, and cna try again. Good luck xx
Thanks everyone - I thought I had put it back in the flame for long enough but obviously not. I even encased with stringer as it seemed slightly faster. Next time I'll heat the bejesus out of it!
Its a gutter having something that you are really pleased with you break or crack isn't it??
Loving the colours in the one that broke..... :( try and make it again tomorrow???
Funnily enough, I was just mourning it before I read your post - you've inspired me to do it again, thanks for that! ;D
I had a focal break on me last weekend and I could have cried.....it was made with either Nyx or Psyche (can't remember now) and encased with clear and for some reason I had managed to get the post wonderful peacock blues out of the DH and encased it just right, capuring all the shine. It fell in half when I tried to get it off the mandrel.
I sat looking at it for about 20 minutes, wondering whether I should try supergluing it together but in the end i chucked it into my pot of bead release, so at least it is still being useful as a bead release mixer if it isn't being pretty anymore!
Look forward to seeing your next attempt.
I find it's usually the area at the holes that needs the heat, and it's the easiest part to miss!
Fruddy, rescue your broken bead, clean it up and then slump it into a pair of cabs in the kiln. Waste not, want not ;D
Am I right in thinking that thermal cracking of glass will do it there and then and a COE problem will do it then, 5 mins later or even years down the line.
I reckon it was a COE problem. . Maybe it was that?
A COE problem would crack like crazy paving - if that makes sense!
Definitely not a COE problem - I keep my different coe's in different rooms! Better safe than sorry. ;D
Quote from: Hotglass28 on October 27, 2010, 11:57:16 AM
Am I right in thinking that thermal cracking of glass will do it there and then and a COE problem will do it then, 5 mins later or even years down the line.
Not necessarily. Or, at least, thermal cracks can be there but not visible until they've widened later.
Even if you have one COE, colours, and batches can alter the COE very very slightly. So it might still be a COE problem. This of course is also different with every manufacturer.
Somewhere there is the techno geekery article about in depth explanations on what goes on with COE and the myths. Cant remember where now?
How about trying it again using exactly the same glass in roughly the same amounts, the same way you did it before and veiwing it under a polarising lens?
Denise
Was it Dennis Brady who said in his PDF that just because mixing of coes has been done 100's of times doesnt mean there is a problem.
http://www.warmglass.com/Glass_compatibility.htm
This wasn't the one I was on about but a start.
I think I may buy a polarising lens from Sam - I'm a little concerned about whether or not my kiln is correctly annealing so it may be an idea to check that they are safe for use. I keep meaning to and never get round to it, but feel I should now. I try not to mix my manufacturers too much, especially for large beads, but sometimes just can't get the colours I want otherwise. I think this was effetre and CIM, so I may try the same bead with a similar CIM colour - not effetre, I only have 004 clear.