Frit-Happens !

Lampwork => COE 104 => Topic started by: ShinySnail on August 17, 2010, 01:58:00 PM

Title: Pinks Cracking
Post by: ShinySnail on August 17, 2010, 01:58:00 PM
I had a pink session last night, and made a few beads using Gold Violet, Gold Ruby and Pink Lady.

When I peeked into my bubbles this morning pretty much everything had cracked!
I was mainly using them over white, adding a little decoration and not encasing.
I should be getting a kiln soon, will this be the answer to all my pink problems?

While I'm here, I was treating the Gold Violet and Gold Ruby as I would Rubino... (because of the 'gold' bit!)
Do I need to?

Thanks,
Anna
Title: Re: Pinks Cracking
Post by: Trudi on August 17, 2010, 02:23:20 PM
There shouldn't be any reason at all.

Did you let them cool too much before you put them on the bubbles? What were the crack like? Straight down the holes?
Title: Re: Pinks Cracking
Post by: ShinySnail on August 17, 2010, 03:47:46 PM
Hi Trudi,
I don't normally have this problem with other colours, the cracks are straight up the sides as though they could break in half.

I didn't really hang about before putting them into the bubbles, but I'm not very experienced so perhaps I was working them too cool using my Rubino theory... I have only ever used Rubino once before and though I got a lovely colour that bead broke in half too.

hmmm maybe that's it, perhaps I need to be a bit less scared of getting the pink glass too hot!
Title: Re: Pinks Cracking
Post by: Trudi on August 17, 2010, 03:51:33 PM
Hi

This does sound like a thermal crack. Rubino doesn't like a reduction flame - it works better in an oxidising one. So if you're on a hot head you're better working further out in the flame. But you should be able to give them a good heat (not cook!).

NB - that all being the rule, I did have a batch of Rubino that when heated more gave a more golden/brown colour. But with these fancy glass's they will vary from batch to batch sometimes!

Hope that helps!

Trudi x
Title: Re: Pinks Cracking
Post by: ShinySnail on August 17, 2010, 04:22:29 PM
Ok thanks, I think it deff sounds like I'm doing something wrong here then!
Will have a play and see how it goes - I'm using a minor but have been working far out in the flame to try to keep the bead as cool as poss so perhaps this is why

Thanks for you help   :)
Title: Re: Pinks Cracking
Post by: Trudi on August 17, 2010, 05:33:16 PM
No worries - don't be afraid of the glass, and just control the flame by adjusting either the oxygen or propane!