Frit-Happens !

Lampwork => COE 104 => Topic started by: helbels on October 04, 2009, 04:53:19 PM

Title: Triton on a HH - how to get silver appearance?
Post by: helbels on October 04, 2009, 04:53:19 PM
Hello all

Yes It's only Day 5 for me, and I know I shouldn't even be going near Triton yet, but I couldn't resist!

I've managed to reduce it, but I'm only getting gold tones coming from it.  How do I get silver?  Do I need to waft it in the flame for a lot longer than I'm currently doing??

Thank you

Helen
Title: Re: Triton on a HH - how to get silver appearance?
Post by: TillyBean on October 04, 2009, 06:55:10 PM
Not sure if it will work but have you tried the Tin foil around the holes at the top of the hot head.. Martin from Tuffnells showed me this at a Bead Fair!  :)

Apologies if you have already tried this..

If not when you try watch your fingy's cos the foil gets very hot!   :o

Gail X
Title: Re: Triton on a HH - how to get silver appearance?
Post by: Mary on October 04, 2009, 07:32:28 PM
If you are getting gold you are reducing it too far. Are you using the tin-foil collar, or using the blue cones? I think the blue cones are too hot, I could never use them well. Try the tin-foil collar, and reduce in the tip of the flame, at arm's length. And very briefly. You can repeat a few times if you need to.
Title: Re: Triton on a HH - how to get silver appearance?
Post by: helbels on October 04, 2009, 07:39:10 PM
I'm using the slightly lesser known technique of... cover the holes on the HH with the strap of my leather apron  ;D ;D ;D ;D  It's a bit Heath Robinson but it works, and is less burny on the fingers!!

It seems it is doing too good a job - I will literally just waft it in there next time - I've been holding it there for a minute or so!
Title: Re: Triton on a HH - how to get silver appearance?
Post by: Mary on October 04, 2009, 07:49:33 PM
Yep, too much! It's hard to explain, but really just a second or two. Then again if you need it. I tend to get silver first, then rainbow colours, then the gold. You can go back into a normal flame if you go too far and melt it off a bit.
Title: Re: Triton on a HH - how to get silver appearance?
Post by: helbels on October 04, 2009, 08:00:58 PM
Thanks Mary, you are a star  ;D