Lampwork => COE 104 => Topic started by: Kaz on June 12, 2009, 11:24:07 PM

Title: CIM clear + Silver Glass = NoNo!?
Post by: Kaz on June 12, 2009, 11:24:07 PM
Just picked up two lentil beads on my desk that I was really pleased with - only to spot that both have cracked completely (in straight lines but not down the middle). I thought I had used effetre 006 but I think I must have picked up the rod of CIM clear that I had been trying out for standard encasing by mistake. Anyone else tried CIM with silver glass?
Bum!
Kazx
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: Sarah on June 12, 2009, 11:37:35 PM
Hi Kaz

I've used it without any problems.

But I have had problems with a stoneground/pysche/effetre crystal clear combination. If I remember rightly it was a stoneground base with effetre cc over pysche bumps.

Sarah
xxx
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: sarah t on June 12, 2009, 11:47:58 PM
bugger about your beads............ but nice to know it happens to the best makers too !!
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: sea-thistle on June 12, 2009, 11:57:24 PM
I made some beads with CIM Celadon and it was really shocky! Glass flying everywhere, and the rod cracking! :(
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: Calico Cat on June 13, 2009, 08:02:16 AM
Quote from: sea-thistle on June 12, 2009, 11:57:24 PM
I made some beads with CIM Celadon and it was really shocky! Glass flying everywhere, and the rod cracking! :(

**!**! I've just treated myself to a load of Celadon 'cause I love the colour . .  thanks for the warning - have to be careful  :)

Carole
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: Shirley on June 13, 2009, 08:04:28 AM
I have used crocus, psyche and encased with Lauscha with no problems at all. The bead was a kalera too, so pressing it was fine.
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: sea-thistle on June 13, 2009, 11:46:58 AM
I love the celadon colour too Carole, it's beautiful! - Karin
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: GoodMonkey on June 13, 2009, 11:56:59 AM
I used Celadon on top of silvered ivory and it sort of pinged itself off wherever it touched the SI.
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: Trudi on June 13, 2009, 01:21:29 PM
i think that celadoncan be a bit of a diva - doesn't like to be encased (at least not by me!!)
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: saffie on June 13, 2009, 01:28:00 PM
Not tried CiM with silver glass but I encased some beads made with base of Northstar sasha silver and with some lausha last night and the sasha silver has gone a pooey brown!!! Yuk!!!
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: Helen G on June 13, 2009, 04:55:49 PM
I did Anouk's "Making Silver Glass Sing" tutorials using CIM clear and didn't have any cracking...............yet  :-\
Title: Re: CIM clear + Silver Glass = NoNo!?
Post by: Hayley on July 02, 2009, 07:33:29 PM
It depends on when you purchased your CiM Clear. When it first came out early 2008, there was compatibility issue with silver glass. Kathy from CiM assured us that they would test with silver glass since so I believe the recent batches are compatible.